# US 2016/0144946 A1 · Extrados structural element made from an aluminium copper lithium alloy

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2016/0144946 A1
- Document ID: US20160144946A1
- Status: Published application
- Kind: A1
- Application number: 14/899,743
- Filed: 2014-06-18
- Published: 2016-05-26
- Earliest claimed: 2013-07-21
- Assignees: Constellium Issoire
- Applicants: Constellium Issoire
- Inventors: Armelle DANIELOU; Gaelle POUGET; Christophe SIGLI
- Web page: https://patentgrep.com/patent/US20160144946A1

## CPC

- B64C 3/26: Construction, shape, or attachment of separate skins, e.g. panels
- B22D 21/007: {with low melting point, e.g. Al 659 degrees C, Mg 650 degrees C}
- C21D 1/30: Stress-relieving
- C21D 8/00: Modifying the physical properties of ferrous metals or ferrous alloys by deformation combined with, or followed by, heat treatment (hardening articles or materials formed by forging or rolling with no further heating beyond that required for the formation C21D1/02)
- C22C 1/026: {Alloys based on aluminium}
- C22C 21/12: with copper as the next major constituent
- C22C 21/14: with silicon
- C22C 21/16: with magnesium
- C22F 1/057: of alloys with copper as the next major constituent
- B64C: AEROPLANES; HELICOPTERS
- B22D: CASTING OF METALS; CASTING OF OTHER SUBSTANCES BY THE SAME PROCESSES OR DEVICES (shaping of plastics or substances in a plastic state B29C; metallurgical processing, selection of substances to be added to metal C21, C22)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)

## Abstract

The invention relates to an extrados structural element made from an aluminum, copper and lithium alloy and a method for manufacturing same. In the method according to the invention, an alloy with composition (in wt %) 4.2 to 5.2 Cu, 0.9 to 1.2 Li, 0.1 to 0.3 Ag, 0.1 to 0.25 Mg, 0.08 to 0.18 Zr, 0.01 to 0.15 Ti, optionally up to 0.2 Zn, optionally up to 0.6 Mn, an Fe and Si content level less than or equal to 0.1% each, and other element with a content level less than or equal to 0.05% each and 0.15% in total, the aluminum is poured, homogenized, deformed hot and optionally cold, placed in a solution at a temperature of at least 515° C., pulled from 0.5 to 5% and annealed. The combination in particular of the magnesium, copper and manganese content with the temperature in solution can reach a very advantageous elasticity under compression limit. Thus, the products according to the invention having a thickness of at least 12 mm have an elasticity under compression limit in the longitudinal direction of at least 645 MPa and an elongation in the longitudinal direction of at least 7%.

## Claims

### Claim 1

A method for manufacturing an extruded, rolled and/or forged product made of an alloy containing aluminium, said method comprising
a) preparing a molten metal bath comprising 4.2 to 5.2% Cu by weight, 0.9 to 1.2% Li by weight, 0.1 to 0.3% Ag by weight, 0.1 to 0.25% Mg by weight, 0.08 to 0.18% Zr by weight, 0.01 to 0.15% Ti by weight, optionally up to 0.2% Zn by weight, optionally up to 0.6% Mn by weight, a Fe and Si content less than or equal to 0.1% by weight each, other elements with a content less than or equal to 0.05% by weight each and 0.15% by weight total, and the rest of aluminium;
b) a rough shape is cast from said molten metal bath;
c) said shape is homogenized by a heat treatment in which the temperature at mid-thickness of the rough shape reaches at least 510° C. for at least 10 hours,
d) said rough shape is hot worked and optionally cold worked, then homogenized into an extruded, roll and/or forged product;
e) said product is solution heat treated at a temperature of at least 515° C. and quenched;
f) said product undergoes controlled stretching with a permanent set of 0.5 to 5%;
g) said product is aged by heating to a temperature of 140 to 170° C. for 5 to 70 hours.

### Claim 2 (depends on 1)

The method according to claim 1, wherein the copper content of said molten metal bath lies between 4.3 and 5.0% by weight and optionally between 4.4 and 4.8% by weight.

### Claim 3 (depends on 1)

The method according to claim 1, wherein the lithium content of said molten metal bath lies between 1.0 and 1.15% by weight and optionally between 1.03 and 1.10% by weight.

### Claim 4 (depends on 1)

The method according to claim 1, wherein the magnesium content of said molten metal bath lies between 0.15 and 0.24% by weight.

### Claim 5 (depends on 1)

The method according to claim 1, wherein the manganese content of said molten metal bath lies between 0.2 and 0.5% by weight and optionally between 0.3 and 0.45% by weight.

### Claim 6 (depends on 1)

The method according to claim 1, wherein the silver content of said molten metal bath lies between 0.15 and 0.25% by weight.

### Claim 7 (depends on 1)

The method according to claim 1, wherein the zirconium content of said molten metal bath lies between 0.11 and 0.18% by weight and optionally between 0.13 and 0.17% by weight.

### Claim 8 (depends on 1)

The method according to claim 1 wherein the solution heat-treatment temperature is at least 520° C. and optionally at least 522° C.

### Claim 9 (depends on 1)

The method according to claim 1 wherein stress relieving by controlled stretching is performed with a permanent set less than 2% and optionally from 0.5 to 1.5%.

### Claim 10 (depends on 1)

An extruded, rolled and/or forged product made of aluminium alloy obtained by the method according to claim 1, having a thickness of at least 12 mm, a compressive yield stress in the longitudinal direction of at least 645 MPa and an elongation in the longitudinal direction of at least 7%.

### Claim 11 (depends on 10)

The extruded product according to claim 10 comprising a compressive yield stress in the L direction which is at least 680 MPa, a tensile yield stress in the L direction of at least 680 MPa and a fracture toughness KQ(T-L), of at least 17 MPa√m.

### Claim 12 (depends on 11)

The extruded product according to claim 11 wherein the manganese content of which is between 0.2 and 0.5% and wherein said extruded product comprises a compressive yield stress in the direction L of at least 720 MPa, a tensile yield stress in the L direction of at least 710 MPa and a fracture toughness KQ(T-L) of at least 18 MPa√m.

### Claim 13 (depends on 10)

The product according to claim 10, wherein the product is rolled and has a thickness of at least 20 mm, a compressive yield stress in the L direction of at least 650 MPa and a fracture toughness KQ(L-T), of at least 18 MPa√m.

### Claim 14 (depends on 13)

The rolled product according to claim 13, the manganese content of which is between 0.2 and 0.5% by weight, comprising a compressive yield stress in the L direction of at least 653 MPa and optionally at least 655 MPa and a fracture toughness KQ(L-T), of at least 20 MPa√m and optionally at least 24 MPa√m.

### Claim 15 (depends on 10)

An upper wing skin structural element incorporating at least one product according to claim 10 and/or manufactured from said product.