The invention also concerns a binder for an injection moulding composition including: from 35 to 54% by volume of a polymeric base, from 40 to 55% by volume of a mixture of waxes, and approximately 10% by volume of a surfactant, wherein the polymeric base contains copolymers of ethylene and methacrylic or acrylic acid, or copolymers of ethylene and vinyl acetate, or copolymers of ethylene including maleic anhydride or a mixture of these copolymers, as well as polyethylene, polypropylene and acrylic resin.
Claims12
1-12 (canceled)
An injection molding composition selected from the group consisting of compositions (A)-(J):
- (A) an injection molding composition consisting of, by weight:
- 86% of a black zirconium oxide powder, and
- 14% of a binder having a volumetric composition of:
- 24% of HD polyethylene;
- 10% of polypropylene;
- 4% of a copolymer of ethylene and methacrylic acid, comprising 6.5% wt of methacrylic acid;
- 10% of an isobutyl methacrylate polymer resin having a molecular weight of 195,000;
- 1% of an n-butyl and isobutyl methacrylate copolymer resin having a molecular weight of 195,000;
- 11% of Carnauba wax;
- 31% of a paraffin wax;
- 6% of N, N′ ethylene-bis(stearamide);
- and
- 3% of a mixture of stearic acid and palmitic acid;
- (B) an injection molding composition consisting of, by weight:
- 86% of a white zirconium oxide powder, and
- 14% of a binder having a volumetric composition of:
- 26% of HD polyethylene;
- 10% of polypropylene;
- 4% of a copolymer of ethylene and methacrylic acid;
- 11% of an isobutyl methacrylate polymer resin having a molecular weight of 195,000;
- 1% of an n-butyl and isobutyl methacrylate copolymer resin having a molecular weight of 195,000;
- 11% of Carnauba wax;
- 29% of a paraffin wax;
- and
- 8% of N, N′ ethylene-bis(stearamide);
- (C) an injection molding composition consisting of, by weight:
- 86% of an Al2O3 powder, and
- 14% of a binder having a volumetric composition of:
- 26% of HD polyethylene;
- 6% of polypropylene;
- 3.5% of a copolymer of ethylene and methacrylic acid, comprising 6.5% wt of methacrylic acid;
- 6% of an isobutyl methacrylate polymer resin having a molecular weight of 195,000;
- 1% of an n-butyl and isobutyl methacrylate copolymer resin having a molecular weight of 195,000;
- 12% of Carnauba wax;
- 35% of a paraffin wax;
- 5.5% of N, N′ ethylene-bis(stearamide);
- and
- 5% of a mixture of stearic acid and palmitic acid;
- (D) an injection molding composition consisting of, by weight:
- 78% of an Al2O3 powder, and
- 22% of a binder having a volumetric composition of:
- 28% of HD polyethylene;
- 2% of polypropylene;
- 3% of a copolymer of ethylene and methacrylic acid, comprising 6.5% wt of methacrylic acid;
- 5% of an isobutyl methacrylate polymer resin having a molecular weight of 195,000;
- 1% of an n-butyl and isobutyl methacrylate copolymer resin having a molecular weight of 195,000;
- 12% of Carnauba wax;
- 39% of a paraffin wax;
- 5% of N, N′ ethylene-bis(stearamide);
- and
- 5% of a mixture of stearic acid and palmitic acid;
- (E) an injection molding composition consisting of, by weight:
- 90% of a CrC powder, and
- 10% of a binder having a volumetric composition of:
- 24% of HD polyethylene;
- 6% of polypropylene;
- 3% of a copolymer of ethylene and methacrylic acid, comprising 6.5% wt of methacrylic acid;
- 5% of an isobutyl methacrylate polymer resin having a molecular weight of 195,000;
- 1% of an n-butyl and isobutyl methacrylate copolymer resin having a molecular weight of 195,000;
- 12% of Carnauba wax;
- 39% of a paraffin wax;
- 5% of N, N′ ethylene-bis(stearamide);
- and
- 5% of a mixture of stearic acid and palmitic acid;
- (F) an injection molding composition consisting of, by weight:
- 89% of a TiC powder, and
- 11% of a binder having a volumetric composition of:
- 24% of HD polyethylene;
- 6% of polypropylene;
- 3% of a copolymer of ethylene and methacrylic acid, comprising 6.5% wt of methacrylic acid;
- 5% of an isobutyl methacrylate polymer resin having a molecular weight of 195,000;
- 1% of an n-butyl and isobutyl methacrylate copolymer resin having a molecular weight of 195,000;
- 12% of Carnauba wax;
- 39% of a paraffin wax;
- 5% of N, N′ ethylene-bis(stearamide);
- and
- 5% of a mixture stearic acid and palmitic acid;
- (G) an injection molding composition consisting of, by weight:
- 94% of a CW powder, and
- 6% of a binder having a volumetric composition of:
- 25% of HD polyethylene;
- 8% of polypropylene;
- 4% of a copolymer of ethylene and methacrylic acid, comprising 6.5% wt of methacrylic acid;
- 7% of an isobutyl methacrylate polymer resin having a molecular weight of 195,000;
- 1% of an n-butyl and isobutyl methacrylate copolymer resin having a molecular weight of 195,000;
- 11% of Carnauba wax;
- 34% of a paraffin wax;
- 5% of N, N′ ethylene-bis(stearamide);
- and
- 5% of a mixture of stearic acid and palmitic acid;
- (H) an injection molding composition consisting of, by weight:
- 94.5% of a CW powder, and
- 5.5% of a binder having a volumetric composition of:
- 25% of HD polyethylene;
- 8% of polypropylene;
- 4% of a copolymer of ethylene and methacrylic acid, comprising 6.5% wt of methacrylic acid;
- 7% of an isobutyl methacrylate polymer resin having a molecular weight of 195,000;
- 1% of an n-butyl and isobutyl methacrylate copolymer resin having a molecular weight of 195,000;
- 11% of Carnauba wax;
- 37% of a paraffin wax;
- 5% of N, N′ ethylene-bis(stearamide);
- and
- 2% of a mixture of stearic acid and palmitic acid;
- (I) an injection molding composition consisting of, by weight:
- 94% of a W powder, and
- 6% of a binder having a volumetric composition of:
- 26% of HD polyethylene;
- 10% of polypropylene;
- 4% of a copolymer of ethylene and methacrylic acid, comprising 6.5% wt of methacrylic acid;
- 9% of an isobutyl methacrylate polymer resin having a molecular weight of 195,000;
- 1% of an n-butyl and isobutyl methacrylate copolymer resin having a molecular weight of 195,000;
- 11% of Carnauba wax;
- 29% of a paraffin wax;
- 5% of N, N ethylene-bis(stearamide);
- and
- 5% of a mixture of stearic acid and palmitic acid;
- and
- (J) an injection molding composition consisting of, by weight:
- 95% of a W powder, and
- 5% of a binder having a volumetric composition of:
- 25% of HD polyethylene;
- 10% of polypropylene;
- 4% of a copolymer of ethylene and methacrylic acid, comprising 6.5% wt of methacrylic acid;
- 7% of an isobutyl methacrylate polymer resin having a molecular weight of 195,000;
- 1% of an n-butyl and isobutyl methacrylate copolymer resin having a molecular weight of 195,000;
- 11% of Carnauba wax;
- 32% of a paraffin wax;
- 5% of N, N′ ethylene-bis(stearamide);
- and
- 5% of a mixture of stearic acid and palmitic acid.