# US 2015/0144290 A1 · METHOD FOR MANUFACTURING ROUND BILLET OF Ni-CONTAINING HIGH ALLOY HAVING IMPROVED INTERNAL QUALITY

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2015/0144290 A1
- Document ID: US20150144290A1
- Status: Published application
- Kind: A1
- Application number: 14/364,334
- Filed: 2013-08-08
- Published: 2015-05-28
- Earliest claimed: 2012-08-09
- Assignees: Nippon Steel & Sumitomo Metal Corporation
- Applicants: Nippon Steel & Sumitomo Metal Corporation
- Inventors: Seiji Miyamoto; Takayoshi Kagari
- Web page: https://patentgrep.com/patent/US20150144290A1

## CPC

- B22D 11/001: {of specific alloys}
- B22D 11/00: Continuous casting of metals, i.e. casting in indefinite lengths (metal drawing, metal extruding B21C)
- B22D 11/002: {Stainless steels}
- B22D 11/12: Accessories for subsequent treating or working cast stock in situ (rolling immediately subsequent to continuous casting B21B1/46, B21B13/22)
- B22D 11/1206: {for plastic shaping of strands (rolling mills B21B1/46)}
- B22D 11/1213: {for heating or insulating strands}
- C21D 9/0081: {for slabs; for billets}
- C22C 19/055: {with the maximum Cr content being at least 20% but less than 30%}
- C22C 19/056: {with the maximum Cr content being at least 10% but less than 20%}
- C22C 30/00: Alloys containing less than 50% by weight of each constituent
- C22C 30/02: containing copper
- C21D 6/004: {containing Cr and Ni}
- C21D 7/13: by hot working
- B22D: CASTING OF METALS; CASTING OF OTHER SUBSTANCES BY THE SAME PROCESSES OR DEVICES (shaping of plastics or substances in a plastic state B29C; metallurgical processing, selection of substances to be added to metal C21, C22)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

Provided is a method for manufacturing a round billet of Ni-containing high alloy including steps of continuously casting a molten steel by using a casting mold, thereby obtaining a rectangular billet, and shaping the rectangular billet into round billet by forging/rolling, wherein the casting mold has a shape such that a w/h ratio between long side length (w) and short side length (h) of a cross section of the rectangular billet perpendicular to the casting direction of rectangular billet is 1.0 to 2.0, the chemical composition of molten steel is, by mass %: C: 0.005 to 0.250%, Si: 0.05 to 2.00%, Mn: 0.05 to 3.00%, P: 0.04% or less, S: 0.004% or less, Cu: 0.01 to 3.00%, Cr: 10 to 35%, Ni: 10 to 80%, Mo: 1.5 to 10.0%, Al: 0.001 to 0.300%, N: 0.001 to 0.300%, W: 0.00 to 6.00%, Ti: 0.00 to 2.00%, and the balance: Fe and impurities.

## Claims

### Claim 1

A method for manufacturing a round billet of NI-containing high alloy, the method comprising the steps of:
continuously casting a molten steel by means of a casting mold, thereby obtaining a rectangular billet; and
shaping the rectangular billet into a round billet by forging or rolling,
wherein the casting mold has a shape such that a w/h ratio between long side length (w) and short side length (h) of a cross section of the rectangular billet is 1.0 to 2.0, and the cross section is perpendicular to the casting direction of the rectangular billet;
the chemical composition of the molten steel is:
C: 0.005 to 0.250% by mass,
Si: 0.05 to 2.00% by mass,
Mn: 0.05 to 3.00% by mass,
P: no more than 0.04% by mass,
S: no more than 0.004% by mass,
Cu: 0.01 to 3.00% by mass,
Cr: 10 to 35% by mass,
Ni: 10 to 80% by mass,
Mo: 1.5 to 10.0% by mass,
Al: 0.001 to 0.300% by mass,
N: 0.001 to 0.300% by mass,
W: 0.00 to 6.00% by mass,
Ti: 0.00 to 2.00% by mass, and
the balance: Fe and impurities;
a Mo segregation degree of the round billet is no more than 0.20; and
the Mo segregation degree is a ratio ((cMo′−cMo)/cMo) of a difference (cMo′−cMo) between Mo concentration at the axial center of the round billet (cMo′) and Mo concentration in the molten steel (cMo) to Mo concentration in the molten steel (cMo).

### Claim 2 (depends on 1)

The method for manufacturing a round billet of Ni-containing high alloy according to claim 1,
wherein the w/h ratio is 1.0 to 1.7.

### Claim 3 (depends on 1)

The method for manufacturing a round billet of Ni-containing high alloy according to claim 1,
wherein the chemical composition of the molten steel contains:
W: 0.01 to 6.00% by mass.

### Claim 4 (depends on 1)

The method for manufacturing a round billet of Ni-containing high alloy according to claim 1,
wherein the chemical composition of the molten steel contains:
Ti: 0.05 to 2.00% by mass.

### Claim 5 (depends on 1)

The method for manufacturing a round billet of Ni-containing high alloy according to claim 1,
wherein a ratio (A/B) of the cross section of the rectangular billet before the shaping step (A) to the cross section of the round billet after the shaping step (B) is 2.5 to 12.0.

### Claim 6 (depends on 1)

The method for manufacturing a round billet of Ni-containing high alloy according to claim 1,
wherein the shaping step includes soaking the rectangular billet at 1200 to 1300° C. before the forging or rolling; and
the soaking time of the rectangular billet in the soaking step is no less than 9 hours where the shaping is carried out by forging, and is no less than 24 hours where the shaping is carried out by rolling.