# US 2015/0144231 A1 · High strength cold-rolled steel sheet and manufacturing method therefor

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2015/0144231 A1
- Document ID: US20150144231A1
- Status: Published application
- Kind: A1
- Application number: 14/400,453
- Filed: 2013-05-29
- Published: 2015-05-28
- Earliest claimed: 2012-05-31
- Assignees: Kabushiki Kaisha Kobe Seiko Sho (Kobe Steel, Ltd.)
- Applicants: Kabushiki Kaisha Kobe Seiko Sho (Kobe Steel, Ltd.)
- Inventors: Tomokazu Masuda; Katsura Kajihara; Toshio Murakami; Masaaki Miura; Muneaki Ikeda
- Web page: https://patentgrep.com/patent/US20150144231A1

## CPC

- C22C 38/38: with more than 1.5% by weight of manganese
- C21D 1/18: Hardening (C21D1/02 takes precedence); Quenching with or without subsequent tempering (quenching devices C21D1/62)
- C21D 8/0226: {Hot rolling}
- C21D 8/0236: {Cold rolling}
- C21D 8/0263: {following hot rolling}
- C21D 8/1272: {Final recrystallisation annealing}
- C21D 9/46: for sheet metals
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/005: {containing rare earths, i.e. Sc, Y, Lanthanides}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/08: containing nickel {(C22C38/105 takes precedence)}
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/16: containing copper
- C22C 38/18: containing chromium
- C22C 38/34: with more than 1.5% by weight of silicon
- C21D 1/25: Hardening, combined with annealing between 300 degrees Celsius and 600 degrees Celsius, i.e. heat refining ("Vergüten")
- C21D 2211/002: Bainite
- C21D 2211/005: Ferrite
- C21D 2211/008: Martensite
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)

## Abstract

In a steel sheet having a specific chemical composition and having a microstructure including ferrite that is a soft first phase by 20-50% in terms of the area ratio, the remainder being tempered martensite and/or tempered bainite that is a hard second phase, the microstructure of steel of a surface layer section of the steel sheet from the surface to the depth of 100 μm and a center section of t/4-3t/4 (t is the sheet thickness) is controlled.

## Claims

### Claim 1

A cold-rolled steel sheet, comprising:
C: 0.05-0.30 mass %;
Si: 3.0 mass % or less, (exclusive of 0) mass %;
Mn: 0.1-5.0 mass %;
P: 0.1 mass % or less, (exclusive of 0) mass %;
S: 0.02 mass % or less, (exclusive of 0) mass %;
Al: 0.01-1.0 mass %; and
N: 0.01 mass % or less, (exclusive of 0) mass % respectively; iron and inevitable impurities,
wherein
a microstructure comprises ferrite that is a soft first phase by 20-50% in terms of area ratio, and tempered martensite, tempered bainite, or both, that is a hard second phase;
a difference between area ratio Vαs of ferrite of a steel sheet surface layer section from a steel sheet surface to a depth of 100 μm and area ratio Vαc of ferrite of a center section of t/4-3t/4 ΔVα=Vαs−Vαc is less than 10%, where t is a sheet thickness; and
a ratio of hardness Hvs of the steel sheet surface layer section and hardness Hvc of the center section RHv=Hvs/Hvc is 0.75-1.0.

### Claim 2

A cold-rolled steel sheet comprising:
C: 0.05-0.30 mass %;
Si: 3.0 mass % or less, (exclusive of 0) mass %;
Mn: 0.1-5.0 mass %;
P: 0.1 mass % or less, (exclusive of 0) mass %;
S: 0.02 mass % or less, (exclusive of 0) mass %;
Al: 0.01-1.0 mass %; and
N: 0.01 mass % or less, (exclusive of 0) mass % respectively iron and inevitable impurities, wherein
a microstructure comprises ferrite that is a soft first phase by 20-50% in terms of area ratio, and tempered martensite, tempered bainite, or both, that is a hard second phase;
a difference between area ratio Vαs of ferrite of a steel sheet surface layer section from a steel sheet surface to a depth of 100 μm and area ratio Vαc of ferrite of a center section of t/4-3t/4 ΔVα=Vαs−Vαc is 10-50%, where t is a sheet thickness; and
an average grain size of ferrite of the steel sheet surface layer section is 10 μm or less.

### Claim 3 (depends on 1)

The steel sheet according to claim 1, further comprising at least one group selected from groups (a)-(c):
(a) Cr: 0.01-1.0 mass %,
(b) at least one element selected from the group consisting of Mo: 0.01-1.0 mass %, Cu: 0.05-1.0 mass %, and Ni: 0.05-1.0 mass %, and
(c) at least one element selected from the group consisting of Ca: 0.0001-0.01 mass %, Mg: 0.0001-0.01 mass %, Li: 0.0001-0.01 mass %, and REM: 0.0001-0.01 mass %.

### Claim 4 (depends on 1)

A method of manufacturing the cold-rolled steel sheet according to claim 1, comprising hot rolling, thereafter cold rolling, thereafter annealing, and tempering with respective conditions (A1)-(A4):
(A1) hot rolling condition:
finish rolling temperature: Ar3 point or above
coiling temperature: above 600° C. and 750° C. or below;
(A2) cold rolling condition:
cold rolling ratio: more than 50% and 80% or less;
(A3) annealing condition:
holding at an annealing temperature of Ac1 or above and below (Ac1+Ac3)/2 for annealing holding time of 3,600 s or less, thereafter slow cooling with a first cooling rate of 1° C./s or more and less than 50° C./s from the annealing temperature to a first cooling completion temperature of 730° C. or below and 500° C. or above, and thereafter rapid cooling with a second cooling rate of 50° C./s or more to a second cooling completion temperature of Ms point or below; and
(A4) tempering condition:
tempering temperature: 300-500° C.
tempering holding time: 60-1,200 s within the temperature range of 300° C.-tempering temperature.

### Claim 5 (depends on 2)

A method of manufacturing the cold-rolled steel sheet according to claim 2, comprising hot rolling, thereafter pickling, cold rolling, thereafter annealing, and tempering with respective conditions (B1)-(B4):
(B1) hot rolling condition:
finish rolling temperature: Ar3 point or above
coiling temperature: 600-750° C.;
(B2) cold rolling condition:
cold rolling ratio: 20-50%
(B3) annealing condition:
holding at an annealing temperature of (Ac1+Ac3)/2−Ac3 for annealing holding time of 3,600 s or less, thereafter slow cooling with a first cooling rate of 1° C./s or more and less than 50° C./s from the annealing temperature to a first cooling completion temperature of 730° C. or below and 500° C. or above, and thereafter rapid cooling with a second cooling rate of 50° C./s or more to a second cooling completion temperature of Ms point or below; and
(B4) tempering condition:
tempering temperature: 300-500° C.
tempering holding time: 60-1,200 s within the temperature range of 300° C.-tempering temperature.