# US 2015/0102476 A1 · Quad flat no lead package and production method thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2015/0102476 A1
- Document ID: US20150102476A1
- Status: Published application
- Kind: A1
- Application number: 14/367,788
- Filed: 2012-08-31
- Published: 2015-04-16
- Earliest claimed: 2012-08-31
- Assignees: Huatian Technology (Xi'an) Co., Ltd.; Tianshui Huatian Technology Co., Ltd.
- Inventors: Wenhui Zhu; Wei Mu; Zhaoming Xu; Xiaowei Guo
- Web page: https://patentgrep.com/patent/US20150102476A1

## CPC

- H10W 70/466: {Tape carriers or flat leads}
- H10W 70/042: {Etching}
- H10W 70/421: {Shapes or dispositions}
- H10W 70/456: {Materials}
- H10W 74/111: {the semiconductor body being completely enclosed}
- H10W 74/114: {by a substrate and the encapsulations}
- H10W 70/457: {of metallic layers on leadframes}
- H10W 72/01561: {Chemical or physical modification, e.g. by sintering or anodisation (patterning H10W72/01551)}
- H10W 72/019: {of bond pads}
- H10W 72/01953: {by etching}
- H10W 72/01971: {Cleaning, e.g. oxide removal}
- H10W 72/07338: {hardening the adhesive by curing, e.g. thermosetting}
- H10W 72/075: {of bond wires}
- H10W 72/07521: {Aligning}
- H10W 72/07554: {changes in dispositions}
- H10W 72/325: {Die-attach connectors having a filler embedded in a matrix}
- H10W 72/352: {comprising metals or metalloids, e.g. solders}
- H10W 72/354: {comprising polymers}
- H10W 72/541: {Dispositions of bond wires}
- H10W 72/547: {Dispositions of multiple bond wires}
- H10W 72/5525: {comprising copper [Cu]}
- H10W 72/884: {Die-attach connectors and bond wires}
- H10W 72/952: {comprising metals or metalloids, e.g. PbSn, Ag or Cu}
- H10W 74/00: Encapsulations, e.g. protective coatings
- H10W 90/736: {between a chip and a stacked lead frame, conducting package substrate or heat sink}
- H10W 90/756: {between a chip and a stacked lead frame, conducting package substrate or heat sink}
- H10W: GENERIC PACKAGES, INTERCONNECTIONS, CONNECTORS OR OTHER CONSTRUCTIONAL DETAILS OF DEVICES COVERED BY CLASS H10

## Abstract

The present invention discloses a quad flat no lead package and a production method thereof. The quad flat no lead package comprises a lead frame carrier consisting of a carrier pit and three circles of leads arranged around the carrier pit, wherein the three circles of leads respectively consist of a plurality of leads that are disconnected mutually; an IC chip is adhered in the carrier pit; and an inner lead chemical nickel and porpezite plated layer is plated on all the leads; the inner lead chemical nickel and porpezite plated layer is arranged in the same direction as the IC chip; the IC chip is connected with the inner lead chemical nickel and porpezite plated layer through a bonding wire; and the IC chip, the ends of all the leads plated with the inner lead chemical plating nickel and palladium metal layers and the bonding wire are all packaged in a plastic package. The quad flat no lead package is manufactured through the following steps of: thinning and scribing a wafer; manufacturing a lead frame; loading the chip; performing pressure welding and plastic packaging; performing post-curing; printing; electroplating; separating the leads; separating a product; and testing/braiding. According to the package, the problems of few leads, long welding wire, high welding cost and limited frequency application during single-face packaging of the existing normal quad flat no lead package are solved.

## Claims

### Claim 1

A quad flat no lead package, comprising a lead frame carrier (1), wherein the lead frame carrier (1) consists of a carrier pit (14) and three circles of leads arranged around the carrier pit (14); the three circles of leads respectively consist of a plurality of leads that are disconnected mutually; an IC chip (3) is adhered in the carrier pit (14); and an inner lead chemical nickel and porpezite plated layer (11) is plated on all the leads; the inner lead chemical nickel and porpezite plated layer (11) is arranged in the same direction as the IC chip (3); the IC chip (3) is connected with the inner lead chemical nickel and porpezite plated layer (11) through a bonding wire; and the IC chip (3), the ends of all the leads plated with the inner lead chemical plating nickel and palladium metal layers (11) and the bonding wire are all packaged in a plastic package body (15).

### Claim 2 (depends on 1)

A production method for a quad flat no lead package according to claim 1, wherein the production method specifically is carried out according to the following steps of:
Step 1: thinning and scribing a wafer, and manufacturing a lead frame;
Adopt an ordinary QFN thinning method to thin a wafer to obtain a wafer having a final thickness of 150 μm˜200 μm, wherein a rough polishing range is from original wafer+adhesive film to final thickness+adhesive film thickness+50 μm, a rough polishing speed is 3 μm/s˜6 μm/s, a fine grinding thickness range is from final thickness+adhesive film thickness+50 μm to final wafer thickness+adhesive film thickness, and a fine grinding speed is 10 μm/min˜20 μm/min; and adopt a breakage-proof process to perform scribing on the thinned wafer to obtain an IC chip, wherein a breakage-proof and anti-cracking scribing process software control technique is adopted, and a scribing feeding speed is ≦10 mm/s;
Manufacturing a lead frame;
First step: take a copper plate having a thickness of 6 mil˜8 mil, pretreat and coarsen the surface of the copper plate, to obtain a lead frame matrix;
Second step: evenly coat photosensitive ink on one surface of the lead frame matrix in a silk screening manner, bake for 10 minutes at a temperature of 75° C.˜80° C. to harden the photosensitive ink; use UV rays to irradiate a negative film, to form a figure on the surface of the lead frame matrix; use a Na2CO3 corrosive liquid having a concentration of 0.8 g/L˜1.2 g/L to treat the photosensitive ink irradiated by the UV rays, to form a discontinuous first photosensitive adhesive layer having a thickness of 10 μm˜15 μm on the surface of the lead frame matrix;
Third step: chemically plate chemical nickel and porpezite on the surface region of the lead frame matrix not covered by the first photosensitive adhesive layer, to form an inner lead chemical nickel and porpezite plated layer having a thickness of 0.5 μm˜5 μm;
Fourth step: use a sodium hydroxide corrosive liquid having a concentration of 3%˜5% to remove the first photosensitive adhesive layer on the surface of the lead frame matrix, leave the inner lead chemical nickel and porpezite plated layer on the surface of the lead frame matrix, and wash;
Fifth step: plate photosensitive ink on the surface of the lead frame matrix having the inner lead chemical nickel and porpezite plated layer, to form a second photosensitive adhesive layer having a thickness of 10 μm˜20 μm on the surface of the inner lead chemical nickel and porpezite plated layer, wherein the plating method and subsequent treatment method are the same as the second step;
Sixth step: use a ferric trichloride to perform half-corrosion on the surface of the lead frame matrix having the second photosensitive adhesive layer, wherein the region of the area not covered by the second photosensitive adhesive layer is corroded by the ferric trichloride etching liquid, and a corrosion depth is 0.06 mm+/−5 μm; form a carrier pit, a plurality of first inner leads, a plurality of second inner leads and a plurality of third inner leads in the surface, wherein the plurality of first inner leads form a first circle of inner leads; the plurality of second inner leads form a second circle of inner leads, and the plurality of third inner leads form a third circle of inner leads;
Seventh step: use a sodium hydroxide corrosive liquid to remove the second photosensitive adhesive layer, and wash, to obtain a lead frame;
Step 2: loading the chip;
Adhere the IC chip on the bottom surface of the carrier pit; cure after the chip is completely loaded, and adopt an ESPEC to bake for 3 h+0.5 h through a delamination resistance process, wherein a baking temperature is 175° C.+/−5° C.;
Step 3: bonding wire from the IC chip to each inner lead of the lead frame;
Step 4: selecting an environment friendly molding compound having a water absorbing capacity ≦0.35%, and an expansion coefficient a1≦1, to carry out plastic packaging and obtain a semifinished product, and adopt an ultra-thin packaging anti-warping process and a multiple-stage molding anti-warping software control technique to carry out wire-deformation prevention and delamination resistance packaging;
Step 5: using an oven which is filled with chlorine gas, ventilates smoothly, is flexible to control temperature, and has a temperature departure smaller than +/−3° C., to perform post-curing on the semifinished product after plastic packaging for 5 h, wherein a post-curing temperature is 150+/−3° C., and a QFN anti-warping curing fixture is adopted during the post-curing process;
Step 6: same with conventional QFN printing;
Step 7: carrying out electroplating and lead separation;
Adopt a high precision high stability metal etching machine to spray the ferric trichloride corrosive liquid to the back side of the lead frame, carry out corrosive thinning on the back side of the lead frame, wherein a corrosive thinning thickness is 0.03 mm˜0.04 mm, and a corrosive thinning precision is controlled within +/−5 μm; use two-stage deionized water to clean the corrosive liquid remained on the surface of the lead frame after corrosion; use a dilute sulfuric acid corrosive liquid or a hydrochloric acid corrosive liquid to activate the surface of the lead frame, and remove oxide on the surface of the lead frame; thoroughly clean corrosive liquid medicine and pickling liquid medicine on the surface of the lead frame through five-stage tap water; dry via strong air and hot air; electroplate a copper layer having a thickness of 8 μm˜10 μm on the surface of the lead frame after corrosive thinning, then electroplate a pure tin layer having a thickness of 7 μm˜15 μm on the surface of the electroplated copper layer, and finally use laser to cut from the back side of the lead frame, to realize lead separation;
Or, electroplate a pure tin layer having a thickness of 7 μm˜15 μm on the back side of the lead frame firstly, then use a blade to cut the back side of the lead frame, wherein a cutting depth is 0.03 mm˜0.04 mm, a cutting depth precision is controlled within +/−5 μm, and a cutting width is 0.2 mm˜0.25 mm; and then use laser to ablate connected parts between the leads, to realize lead separation;
Or, electroplate a pure tin layer having a thickness of 7 μm˜15 μm on the back side of the lead frame firstly, and use a water jet to cut the back side of the lead frame, to realize lead separation;
Step 8: separating a unit product from the frame; and
Step 9: testing/braiding;
The conventional test of the packaging is same as the O/S and open short circuit tests of a traditional QFN product; meanwhile, electrical property and thermal property tests are required so as to ensure the high yield rate and high reliability of the product, and prepare the quad flat no lead package.

### Claim 3 (depends on 2)

The production method according to claim 2, wherein an AD889 loading machine or an AD829 loading machine is adopted to load the chip in step 2.

### Claim 4 (depends on 2)

The production method according to claim 2, wherein an ASM eagle60 wire bonder or a W 3100 plus optima wire bonder is adopted to carry out pressure bonding in step 3.

### Claim 5 (depends on 2)

The production method according to claim 2, wherein “M”-shaped arc, high and low arc or reverse wire bonding is adopted in step 3 so as to ensure no short circuit between the bonding wires.

### Claim 6 (depends on 2)

The production method according to claim 2, wherein a lower spraying manner is adopted to spray the corrosive liquid in step 7, wherein a spraying pressure is 3 bar˜4 bar.

### Claim 7 (depends on 2)

The production method according to claim 2, wherein a high precision solid ultraviolet laser cutting machine is adopted during laser cutting in step.