# US 2015/0101715 A1 · High strength steel wire for spring excellent in coiling performance and hydrogen embrittlement resistance and method for manufacturing same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2015/0101715 A1
- Document ID: US20150101715A1
- Status: Published application
- Kind: A1
- Application number: 14/397,734
- Filed: 2013-05-20
- Published: 2015-04-16
- Earliest claimed: 2012-05-31
- Assignees: Kabushiki Kaisha Kobe Seiko Sho (Kobe Steel, Ltd.)
- Applicants: Kabushiki Kaisha Kobe Seiko Sho (Kobe Steel, Ltd.)
- Inventors: Atsuhiko Takeda; Nao Yoshihara
- Web page: https://patentgrep.com/patent/US20150101715A1

## CPC

- C21D 9/02: for springs
- C21D 1/18: Hardening (C21D1/02 takes precedence); Quenching with or without subsequent tempering (quenching devices C21D1/62)
- C21D 8/06: during manufacturing of rods or wires
- C21D 9/52: for wires; for strips {; for rods of unlimited length}
- C21D 9/525: {for wire, for rods (C21D9/54 takes precedence)}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/08: containing nickel {(C22C38/105 takes precedence)}
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- C22C 38/16: containing copper
- F16F 1/021: {characterised by their composition, e.g. comprising materials providing for particular spring properties (composition and manufacture of clock or watch springs G04B1/145)}
- C21D 2211/008: Martensite
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- F16F: SPRINGS; SHOCK-ABSORBERS; MEANS FOR DAMPING VIBRATION

## Abstract

A steel wire for spring is provided which exhibits high strength even without adding a large amount of alloy elements, and is for obtaining a cold winding spring having excellent coiling performance and improved hydrogen embrittlement resistance. The steel wire for spring is characterized in that C: 0.40-0.65% (mass %), Si: 1.0-3.0%, Mn: 0.6-2.0%, P: 0.015% or less (exclusive of 0%), S: 0.015% or less (exclusive of 0%), and Al: 0.015 percent by mass or less (excluding 0%) of S, and Al: 0.001-0.10% are satisfied, with the remainder consisting of iron and inevitable impurities, tempered martensite: 70 area % or more and retained austenite: 6-15 area % with respect to the total microstructure, the prior austenite grain size number obtained by a method stipulated in JIS G 0551 is No. 10.0 or more, and the tensile strength is 1,900 MPa or more.

## Claims

### Claim 1

A high strength steel wire for spring excellent in coiling performance and hydrogen embrittlement resistance, wherein:
C: 0.40-0.65% (means mass %, hereinafter the same with respect to the chemical composition);
Si: 1.0-3.0%;
Mn: 0.6-2.0%;
P: 0.015% or less (exclusive of 0%);
S: 0.015% or less (exclusive of 0%); and
Al: 0.001-0.10% are satisfied, and the remainder consists of iron and inevitable impurities;
tempered martensite: 70 area % or more, and
retained austenite: 6-15 area % with respect to all microstructures are satisfied;
prior austenite grain size number obtained by a method stipulated in JIS G 0551 is No. 10.0 or more; and
tensile strength is 1,900 MPa or more.

### Claim 2 (depends on 1)

The high strength steel wire for spring according to claim 1, further containing one or more elements selected from the group consisting of:
Cu: 0.05-1.5%; and
Ni: 0.05-1.5%.

### Claim 3 (depends on 1)

The high strength steel wire for spring according to claim 1, further containing one or more elements selected from the group consisting of:
Ti: 0.10% or less (exclusive of 0%);
B: 0.010% or less (exclusive of 0%);
Nb: 0.10% or less (exclusive of 0%);
Mo: 0.5% or less (exclusive of 0%); and
V: 0.3% or less (exclusive of 0%).

### Claim 4 (depends on 1)

A spring obtained using the high strength steel wire for spring according to claim 1.

### Claim 5 (depends on 1)

A method for manufacturing the high strength steel wire for spring excellent in coiling performance and hydrogen embrittlement resistance according to claim 1 comprising the steps of:
using steel satisfying the composition according to claim 1; and
executing quenching and tempering executed after drawing so as to satisfy all of quenching conditions and tempering conditions below.
(Quenching conditions)
Average temperature raising rate (HR1) from 100° C. to heating temperature (T1) for quenching shown below: 40° C./s or more
Heating temperature (T1) for quenching: 850-1,000° C.
Holding time (t1) at heating temperature for quenching: 90 seconds or less
Average cooling rate (CR1) from 300° C. to 80° C. after heating for quenching: 5-30° C./s
(Tempering conditions)
Average temperature raising rate (HR2) from 100° C. to heating temperature (T2) for tempering shown below: 30° C./s or more
Heating temperature (T2) for tempering: 350-550° C.
Holding time (t2) at heating temperature for tempering: 5-90 seconds
Average cooling rate (CR2) from the T2 (however, it is 400° C. when the T2 is 400° C. or above) to 100° C. after heating for tempering: 30° C./s or more