- Published: 2015-04-16
- Earliest claimed: 2012-06-19
- Assignees: Buffalo Armory LLC
- Inventors: John BATISTE; Richard CLARE, JR.; Jack HEINZ; Brent NICHOLSON
- Web page: https://patentgrep.com/patent/US20150101713A1

## CPC

- C21D 9/0068: {for particular articles not mentioned below}
- B23K 10/00: Welding or cutting by means of a plasma
- B23K 31/02: relating to soldering or welding
- B23K 37/0211: {travelling on a guide member, e.g. rail, track}
- B23K 37/0408: {for planar work}
- C21D 1/18: Hardening (C21D1/02 takes precedence); Quenching with or without subsequent tempering (quenching devices C21D1/62)
- C21D 1/22: Martempering
- C21D 1/42: Induction heating
- C21D 1/78: Combined heat-treatments not provided for above
- C21D 6/004: {containing Cr and Ni}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 9/42: for armour plate
- C21D 9/505: {Cooling thereof}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/44: with molybdenum or tungsten
- F42B 12/04: of armour-piercing type
- F42B 33/14: Surface treatment of cartridges or cartridge cases {(F42B33/004 takes precedence)}
- B23K 2101/16: Bands or sheets of indefinite length
- B23K 2101/18: Sheet panels
- B23K 2103/04: Steel {or steel} alloys
- C21D 2211/002: Bainite
- C21D 2211/005: Ferrite
- C21D 2211/008: Martensite
- C21D 2211/009: Pearlite
- Y02P 10/25: Process efficiency
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- B23K: SOLDERING OR UNSOLDERING; WELDING; CLADDING OR PLATING BY SOLDERING OR WELDING; CUTTING BY APPLYING HEAT LOCALLY, e.g. FLAME CUTTING; WORKING BY LASER BEAM
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- F42B: EXPLOSIVE CHARGES, e.g. FOR BLASTING, FIREWORKS, AMMUNITION (explosive compositions C06B; fuzes F42C; blasting F42D)
- Y02P: CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS

## Abstract

A method for forming and treating a steel article of a high strength and ductile alloy. The method includes the steps of providing a starting steel composition for the steel article, preheating the composition, heating the starting material to a peak temperature range in less than forty seconds, holding the heated steel composition at the peak temperature range for between two and sixty seconds, quenching the heated steel composition from the peak temperature range to below 177° C. (350° F.) at a temperature rate reduction of 200 to 3000° C./sec (360 and 5400° F./sec), removing residual quench media from the surface of the quenched steel composition, tempering the quenched steel composition at a temperature of 100 to 704° C. (212 to 1300° F.); and air cooling the tempered steel composition to less than 100° C. (212° F.) to form a steel having desired mechanical properties.

## Claims

### Claim 1

A method for treating a steel article to form a high yield strength and ductile alloy comprising the steps of:
(a) providing a steel composition having a material thickness no greater than 0.5 inches (12.7 mm), having an initial microstructure of at least ferrite and pearlite, and having a composition of, by weight,
carbon between 0.25 and 0.55%,
silicon between 0.15 and 0.35%,
manganese between 0.40 and 1.0%,
chromium between 0.40 and 1.10%,
nickel less than 4.5%,
molybdenum between 0.15 and 0.35%,
sulfur less than 0.040%,
phosphorus less than 0.035%,
balance iron and other elements and compounds in making steel;
(b) preheating the provided steel composition to not more than 594° C. (1100° F.);
(c) heating the preheated steel composition to a peak temperature of between 800° C. (1472° F.) and 1150° C. (2102° F.) in less than forty seconds;
(d) holding the heated steel composition at the peak temperature range for between two and twenty seconds;
(e) quenching the heated steel composition from the peak temperature range to below 177° C. (350° F.) at a temperature rate reduction of between 200 and 3000° C./sec (360-5400° F./sec);
(f) removing residual quench media from the surface of the quenched steel composition;
(g) tempering the quenched steel composition at a temperature from 100° C. to 704° C. (212-1300° F.) for less than ninety minutes; and
(h) air cooling the tempered steel composition to less than 100° C. (212° F.) to form a steel article having at least 80% martensite and up to 5% bainite by weight, a yield strength of at least 160 Ksi (1100 MPa), and a total elongation between 5% and 22%.

### Claim 2 (depends on 1)

The method for treating a steel article as claimed in claim 1 where the air cooled steel composition has a V50 protection ballistic limit at 30° obliquity angle at least 2300 feet per second (701 m/s) with a .30 caliber armor piercing round for a thickness of 0.25 inches (6.35 mm).

### Claim 3 (depends on 1)

The method for treating a steel article as claimed in claim 1, where the air cooled steel composition has a microstructure having no more than 1% bainite by weight.

### Claim 4

A method for treating a steel article to form a high yield strength and ductile alloy comprising the steps of:
(a) providing a steel composition having a material thickness no greater than 0.5 inches (12.7 mm), having an initial microstructure of at least ferrite and pearlite, and having a composition of, by weight,
carbon between 0.25 and 0.55%,
silicon between 0.15 and 0.35%,
manganese between 0.40 and 1.0%,
chromium between 0.40 and 1.10%,
nickel less than 4.5%,
molybdenum between 0.15 and 0.35%,
sulfur less than 0.040%,
phosphorus less than 0.035%,
balance iron and other elements and compounds in making steel;
(b) preheating the provided steel composition to not more than 594° C. (1100° F.);
(c) heating the preheated steel composition to a peak temperature of between 800° C. (1472° F.) and 1150° C. (2102° F.) in less than forty seconds;
(d) holding the heated steel composition at the peak temperature range for between two and twenty seconds;
(e) quenching the heated steel composition from the peak temperature range to below 177° C. (350° F.) at a temperature rate reduction of between 200 and 3000° C./sec (360-5400° F./sec);
(f) removing residual quench media from the surface of the quenched steel composition; and
(g) air cooling the steel composition to less than 100° C. (212° F.) to form a steel article having at least 80% martensite and up to 5% bainite by weight, a yield strength of at least 160 Ksi (1100 MPa), and a total elongation between 5% and 22%.

### Claim 5 (depends on 4)

The method for treating a steel article as claimed in claim 4 where the air cooled steel composition has a V50 protection ballistic limit at 30° obliquity angle at least 2300 feet per second (701 m/s) with a .30 caliber armor piercing round for a thickness of 0.25 inches (6.35 mm).

### Claim 6

A method for treating a steel article to form a high yield strength and ductile alloy comprising the steps of:
(a) providing a steel composition having a material thickness no greater than 0.5 inch (12.7 mm), having an initial microstructure of at least ferrite and pearlite, and having a composition of, by weight,
carbon between 0.25 and 0.55%,
silicon between 0.15 and 0.35%,
manganese between 0.40 and 1.0%,
chromium between 0.40 and 1.10%,
nickel less than 4.5%,
molybdenum between 0.15 and 0.35%,
sulfur less than 0.040%,
phosphorus less than 0.035%,
balance iron and other elements and compounds in making steel;
(b) preheating the provided steel composition to not more than 815° C. (1500° F.);
(c) heating the preheated steel composition to a peak temperature between 800-1150° C. (1472-2102° F.) in less than forty seconds;
(d) holding the heated steel composition at the peak temperature range for between two and twenty seconds;
(e) quenching the heated steel composition to below 177° C. (350° F.) in less than four seconds;
(f) removing residual quench media from the surface of the quenched steel composition;
(g) tempering the quenched steel composition at a temperature between 100° C. and 704° C. (212-1300° F.) for less than ninety minutes; and
(h) air cooling the tempered steel composition to less than 100° C. (212° F.) having a transformed microstructure of at least 80% martensite and up to 5% bainite by weight, a yield strength of at least 160 Ksi (1100 MPa), and a total elongation between 5% and 22%.

### Claim 7 (depends on 6)

The method for treating a steel article as claimed in claim 6, where the air cooled steel composition has a microstructure having no more than 1% bainite by weight.

### Claim 8

A method for treating a steel article to form a high yield strength and ductile alloy comprising the steps of:
(a) providing a steel composition having a material thickness no greater than 0.5 inches (12.7 mm), having an initial microstructure of at least ferrite and pearlite, and having a composition of, by weight,
carbon between 0.25 and 0.55%,
silicon between 0.15 and 0.35%,
manganese between 0.40 and 1.0%,
chromium between 0.40 and 1.10%,
nickel less than 4.5%,
molybdenum between 0.15 and 0.35%,
sulfur less than 0.040%,
phosphorus less than 0.035%,
balance iron and other elements and compounds in making steel;
(b) preheating the provided steel composition to a temperature to not more than 815° C. (1500° F.);
(c) heating the preheated steel composition to a peak temperature of between 800° C. (1472° F.) and 1150° C. (2102° F.) in less than forty seconds;
(d) holding the heated steel composition at the peak temperature range for between two and sixty seconds;
(e) quenching the heated steel composition from the peak temperature range to below 100° C. (212° F.) at a temperature rate reduction of between 200 and 3000° C./sec (360-5400° F./sec);
(f) removing residual quench media from the surface of the quenched steel composition;
(g) tempering the quenched steel composition at a temperature from 100° C. to 704° C. (212-1300° F.) for less than ninety minutes; and
(h) air cooling the tempered steel composition to less than 100° C. (212° F.) to form a steel article having at least 80% martensite and up to 5% bainite by weight, a yield strength of at least 160 Ksi (1100 MPa), and a total elongation between 5% and 22%.

### Claim 9 (depends on 8)

The method for treating a steel article as claimed in claim 8 where the air cooled steel composition has a V50 protection ballistic limit at 30° obliquity angle at least 2300 feet per second (701 m/s) with a .30 caliber armor piercing round for a thickness of 0.25 inches (6.35 mm).

### Claim 10 (depends on 8)

The method for treating a steel article as claimed in claim 8, where the air cooled steel composition has a microstructure having no more than 1% of bainite by weight.

### Claim 11

A method for treating a steel article to form a high yield strength and ductile alloy comprising the steps of:
(a) providing a steel composition having a material thickness no greater than 0.5 inches (12.7 mm), having an initial microstructure of at least ferrite and pearlite, and having a composition of, by weight,
carbon between 0.25 and 0.55%,
silicon between 0.15 and 0.35%,
manganese between 0.40 and 1.0%,
chromium between 0.40 and 1.10%,
nickel less than 4.5%,
molybdenum between 0.15 and 0.35%,
sulfur less than 0.040%,
phosphorus less than 0.035%,
balance iron and other elements and compounds in making steel;
(b) preheating the provided steel composition to not more than 594° C. (1100° F.);
(c) heating the preheated steel composition to a peak temperature between 800-1150° C. (1472-2102° F.) in less than forty seconds;
(d) holding the heated steel composition at the peak temperature range for between two and sixty seconds;
(e) quenching the heated steel composition to below 177° C. (350° F.) in less than four seconds;
(f) removing residual quench media from the surface of the quenched steel composition;
(g) tempering the quenched steel composition at a temperature between 100° C. and 704° C. (212-1300° F.) for less than ninety minutes; and
(h) air cooling the tempered steel composition to less than 100° C. (212° F.) having a transformed microstructure of at least 80% martensite and up to 5% bainite by weight, a yield strength of at least 160 Ksi (1100 MPa), and a total elongation between 5% and 22%.

### Claim 12 (depends on 11)

The method for treating a steel article as claimed in claim 11, where the air cooled steel composition has a microstructure having no more than 1% bainite by weight.

### Claim 13 (depends on 11)

The method for treating a steel article as claimed in claim 11, where the air cooled tempered steel composition has a V50 protection ballistic limit at 30° obliquity angle at least 2300 feet per second (701 m/s) with a .30 caliber armor piercing round for a thickness of 0.25 inches (6.35 mm).

### Claim 14 (depends on 11)

The method for treating a steel article as claimed in claim 11, where the steel composition is heated in step (c) in less than twenty seconds.

### Claim 15 (depends on 11)

The method for treating a steel article as claimed in claim 11, where the heated steel composition is held at the peak temperature range for between two and twenty seconds.

### Claim 16 (depends on 11)

The method for treating a steel article as claimed in claim 11, where the heated steel composition is quenched from the peak temperature range to below 177° C. (350° F.) at a temperature rate reduction of between 200 and 3000° C./sec (360-5400° F./sec).

### Claim 17 (depends on 11)

The method for treating a steel article as claimed in claim 11, where the residual quench media is removed from the surface of the quenched steel composition by at least one of mechanical wiping, blown air, and combinations thereof.

### Claim 18 (depends on 11)

The method for treating a steel article as claimed in claim 11, where the tempering step is performed using a conventional oven.

### Claim 19 (depends on 11)

The method for treating a steel article as claimed in claim 11, where the tempering step is performed using a combination of a conventional oven and an induction heater.

### Claim 20 (depends on 11)

The method for treating a steel article as claimed in claim 11, where the tempering step is performed at between 100° C. (212° F.) and 427° C. (800° F.).

### Claim 21 (depends on 11)

The method for treating a steel article as claimed in claim 11 further comprising the step of, prior to heating the steel composition, welding together two lengths of steel plate along the width with one or more welds to form a continuous series of steel plates.

### Claim 22 (depends on 21)

The method for treating a steel article as claimed in claim 21 where the step of welding includes applying a weave weld bridging between lengths of steel plate across the width of the steel plates.

### Claim 23 (depends on 22)

The method for treating a steel article as claimed in claim 22 with the step of welding includes applying a weave weld bridging between lengths of steel plate in three sections where the center portion of steel plate is done first and the side portions are welded to provide a weave weld across the width of the steel plates.

### Claim 24 (depends on 21)

The method for treating a steel article as claimed in claim 21 where in addition a seam weld is applied over the weave weld across the width of the steel plates.

### Claim 25 (depends on 23)

The method for treating a steel article as claimed in claim 23 where in addition a seam weld is applied over the weave weld across the width of the steel plates.

### Claim 26 (depends on 21)

The method for treating a steel article as claimed in claim 21 where an indicia is applied to the steel plate in advance of the welding step to enable a vision system to identify the location of end portions of lengths of the steel plates for the welding step.

### Claim 27 (depends on 11)

The method for treating a steel article as claimed in claim 11 where the heating step is performed using an induction heater.

### Claim 28 (depends on 11)

The method for treating a steel article as claimed in claim 11 where the quenching step is performed by flowing a quench medium over the steel article at a rate of up to 900 gallons/min (3400 L/min).

### Claim 29 (depends on 28)

The method for treating a steel article as claimed in claim 28 where the quench medium is water.

### Claim 30 (depends on 28)

The method for treating a steel article as claimed in claim 28 where the quenching step is performed in more than 1 second and not more than 20 seconds.

### Claim 31 (depends on 28)

The method for treating a steel article as claimed in claim 28 where after at least step (g) the steel plate is cut into lengths at least at the seams while the steel plate continuously moves along the conveyor.

### Claim 32 (depends on 11)

The method for treating a steel article as claimed in claim 11 where the tempering step is performed using an induction heater.

### Claim 33 (depends on 11)

The method for treating a steel article as claimed in claim 11 where the tempering step is performed at between 100° C. (212° F.) and 704° C. (1300° F.) in a time between 1 and 20 seconds.

### Claim 34 (depends on 11)

The method for treating a steel article as claimed in claim 11 where the steel composition has, by weight,
carbon between 0.25 and 0.40%.

### Claim 35 (depends on 11)

The method for treating a steel article as claimed in claim 11 where the steel composition has, by weight,
carbon between 0.40 and 0.55%.

### Claim 36

A method for treating a steel article to form a high yield strength and ductile alloy comprising the steps of:
(a) providing a steel composition having a material thickness no greater than 0.5 inch (12.7 mm), having an initial microstructure of at least ferrite and pearlite, and having a composition of, by weight,
carbon between 0.25 and 0.55%,
silicon between 0.15 and 0.35%,
manganese between 0.40 and 1.0%,
chromium between 0.40 and 1.10%,
nickel less than 4.5%,
molybdenum between 0.15 and 0.35%,
sulfur less than 0.040%,
phosphorus less than 0.035%,
balance iron and other elements and compounds in making steel;
(b) preheating the provided steel composition to not more than 594° C. (1100° F.);
(c) heating the preheated steel composition to a peak temperature between 800-1150° C. (1472-2102° F.) in less than forty seconds;
(d) holding the heated steel composition at the peak temperature range for between two and sixty seconds;
(e) quenching the heated steel composition to below 177° C. (350° F.) in less than four seconds;
(f) removing residual quench media from the surface of the quenched steel composition; and
(h) air cooling the steel composition to less than 100° C. (212° F.) having a transformed microstructure of at least 80% martensite and up to 5% bainite by weight, a yield strength of at least 160 Ksi (1100 MPa), and a total elongation between 5% and 22%.

### Claim 37 (depends on 36)

The method for treating a steel article as claimed in claim 36, where the air cooled steel composition has a microstructure having no more than 1% bainite, by weight.