# US 2014/0272665 A1 · Ceramic Fuel Cell With Enhanced Flatness And Strength And Methods Of Making Same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2014/0272665 A1
- Document ID: US20140272665A1
- Status: Published application
- Kind: A1
- Application number: 14/206,930
- Filed: 2014-03-12
- Published: 2014-09-18
- Earliest claimed: 2013-03-13
- Assignees: Redox Power Systems, LLC; University of Maryland, College Park
- Applicants: Redox Power Systems, LLC; University of Maryland, College Park
- Inventors: Hee Sung YOON; Eric D. WACHSMAN; Bryan M. BLACKBURN
- Web page: https://patentgrep.com/patent/US20140272665A1

## CPC

- H01M 8/1213: characterised by the electrode/electrolyte combination or the supporting material
- B32B 5/16: characterised by features of a layer formed of particles, e.g. chips, powder {or granules (layer formed of natural mineral particles B32B19/00; layer being formed of wood fibres, chips or particles B32B21/02)}
- B32B 5/30: one layer {being formed of particles, e.g. chips,} granules, powder
- H01M 4/8885: {Sintering or firing}
- B32B 2264/102: Oxide or hydroxide
- B32B 2264/107: Ceramic
- B32B 2307/202: Conductive
- B32B 2307/736: Shrinkable
- B32B 2457/18: Fuel cells
- H01M 4/8835: {Screen printing}
- H01M 4/8857: {Casting, e.g. tape casting, vacuum slip casting}
- H01M 4/9066: {of metal-ceramic composites or mixtures, e.g. cermets}
- H01M 8/126: the electrolyte containing cerium oxide
- H01M 2004/8684: {Negative electrodes}
- H01M 2008/1293: {Fuel cells with solid oxide electrolytes}
- Y02E 60/50: Fuel cells
- Y02P 70/50: Manufacturing or production processes characterised by the final manufactured product
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- B32B: LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION
- Y02P: CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS

## Abstract

Ceramic fuel cells having enhanced flatness and strength are disclosed. The fuel cell can include a half-cell having, in order, a patterned layer, an anode support layer and an electrolyte layer. Methods of making ceramic fuel cells are also provided.

## Claims

### Claim 1

A ceramic fuel cell comprising, in order:
a sintered patterned layer having a first coefficient of thermal expansion;
a sintered anode support layer having a second coefficient of thermal expansion;
a sintered first electrolyte layer having a third coefficient of thermal expansion; and
a cathode layer,
wherein the second coefficient of thermal expansion is not between the first coefficient of thermal expansion and the third coefficient of thermal expansion.

### Claim 2 (depends on 1)

The ceramic fuel cell of claim 1, wherein a thickness of the sintered first electrolyte layer is less than a combined thickness of the sintered patterned layer and the sintered anode support layer.

### Claim 3 (depends on 1)

The ceramic fuel cell of claim 1, wherein a thickness of the sintered patterned layer is at least as great as a thickness of the sintered first electrolyte layer.

### Claim 4 (depends on 1)

The ceramic fuel cell of claim 1, wherein a thickness of the sintered patterned layer is 2 to 1500 microns, a thickness of the sintered anode support layer is 250 to 1500 microns, and a thickness of the sintered first electrolyte layer is 2 to 100 microns.

### Claim 5 (depends on 1)

The ceramic fuel cell of claim 1, wherein a thickness of the sintered first electrolyte layer is between 5 to 30 microns

### Claim 6 (depends on 1)

The ceramic fuel cell of claim 1, wherein the third coefficient of thermal expansion is within twenty five percent of the first coefficient of thermal expansion.

### Claim 7 (depends on 1)

The ceramic fuel cell of claim 1, wherein the third coefficient of thermal expansion is within ten percent of the first coefficient of thermal expansion.

### Claim 8 (depends on 1)

The ceramic fuel cell of claim 1, wherein the third coefficient of thermal expansion is within five percent of the first coefficient of thermal expansion.

### Claim 9 (depends on 1)

The ceramic fuel cell of claim 1, wherein the third coefficient of thermal expansion is within one percent of the first coefficient of thermal expansion.

### Claim 10 (depends on 1)

The ceramic fuel cell of claim 1, wherein the first and third coefficients of thermal expansion are substantially the same.

### Claim 11 (depends on 1)

The ceramic fuel cell of claim 1, wherein the second coefficient of thermal expansion is at least 1 percent different from each of the first and third coefficients of thermal expansion.

### Claim 12 (depends on 1)

The ceramic fuel cell of claim 1, wherein the sintered patterned layer, sintered anode support layer, and sintered first electrolyte layer are fabricated by:
providing a first structure comprising, in order:
a patterned layer comprising, prior to sintering, green bodies having a first composition;
an anode support layer comprising, prior to sintering, green bodies having a second composition; and
a first electrolyte layer comprising, prior to sintering, green bodies having a third composition;
sintering the first structure at a first sintering temperature to obtain the sintered patterned layer, sintered anode support layer, and sintered first electrolyte layer;
wherein, during sintering, the first composition has a first shrinkage, the second composition has a second shrinkage, and the third composition has a third shrinkage; and
the second shrinkage is not between the first shrinkage and the third shrinkage.

### Claim 13 (depends on 12)

The ceramic fuel cell of claim 12, wherein the third shrinkage is within ten percent of the first shrinkage.

### Claim 14 (depends on 12)

The ceramic fuel cell of claim 12, wherein the third shrinkage is within three percent of the first shrinkage.

### Claim 15 (depends on 12)

The ceramic fuel cell of claim 12, wherein the third shrinkage is within one percent of the first shrinkage.

### Claim 16 (depends on 12)

The ceramic fuel cell of claim 12, wherein the first and third shrinkages are equal.

### Claim 17 (depends on 12)

The ceramic fuel cell of claim 12, wherein the second shrinkage is at least one percent different from each of the first shrinkage and the third shrinkage.

### Claim 18 (depends on 12)

The ceramic fuel cell of claim 12, wherein the second shrinkage is between one and ten percent different from each of the first shrinkage and the third shrinkage.

### Claim 19 (depends on 12)

The ceramic fuel cell of claim 12, wherein the patterned layer, the anode support layer, and the first electrolyte layer are not constrained during sintering.

### Claim 20 (depends on 12)

The ceramic fuel cell of claim 12, wherein the patterned layer, the anode support layer, and the first electrolyte layer are constrained during sintering

### Claim 21 (depends on 12)

The ceramic fuel cell of claim 12, further comprising:
after sintering the patterned layer, the anode support layer, and the first electrolyte layer:
providing a second electrolyte layer over the first electrolyte layer, the second electrolyte layer comprising, prior to sintering, green bodies having a fourth composition; and
sintering the second electrolyte layer at a second sintering temperature lower than the first sintering temperature.

### Claim 22 (depends on 12)

The ceramic fuel cell of claim 12, further comprising:
after sintering the patterned layer, the anode support layer, and the first electrolyte layer:
providing a cathode layer over the first electrolyte layer, the cathode layer comprising, prior to sintering, green bodies having a fifth composition; and
sintering the cathode layer at a second sintering temperature lower than the first sintering temperature.

### Claim 23 (depends on 12)

The ceramic fuel cell of claim 12, wherein the first composition comprises GDC, the second composition comprises NiO-GDC, and the third composition comprises GDC.

### Claim 24 (depends on 12)

The ceramic fuel cell of claim 12, wherein the second composition comprises NiO and Ce1-xGdxO2-0.5x powders, and the first and third compositions comprise Ce1-xGdxO2-0.5x powder, wherein 0≦x≦0.2.

### Claim 25 (depends on 12)

The ceramic fuel cell of claim 12, wherein the first composition and the third composition are at least partially made of the same material.

### Claim 26 (depends on 12)

The ceramic fuel cell of claim 12, wherein the first composition and the third composition are the same.

### Claim 27 (depends on 12)

The ceramic fuel cell of claim 12, wherein the first electrolyte layer comprises at least one of yttria stabilized zirconia (YSZ), scandia stabilized zirconia (SSZ), gadolinia doped ceria (GDC), samaria doped ceria (SDC), samarium-neodymium doped ceria (SNDC), strontium and magnesium doped lanthanum gallate (LSGM), and combinations of multiple dopants and stabilizers in these electrolytes.

### Claim 28 (depends on 12)

The ceramic fuel cell of claim 12, wherein the anode support layer comprises a composite anode comprised of NiO and one or more of yttria stabilized zirconia (YSZ), scandia stabilized zirconia (SSZ), gadolinia doped ceria (GDC), samaria doped ceria (SDC), samarium-neodymium doped ceria (SNDC), strontium and magnesium doped lanthanum gallate (LSGM), and combinations of multiple dopants and stabilizers in these materials.

### Claim 29 (depends on 12)

The ceramic fuel cell of claim 12, wherein the patterned layer comprises at least one of yttria stabilized zirconia (YSZ), scandia stabilized zirconia (SSZ), gadolinia doped ceria (GDC), samaria doped ceria (SDC), samarium-neodymium doped ceria (SNDC), strontium and magnesium doped lanthanum gallate (LSGM), and combinations of multiple dopants and stabilizers in these materials.

### Claim 30 (depends on 1)

The ceramic fuel cell of claim 1, wherein the patterned layer comprises one or more apertures.

### Claim 31 (depends on 1)

The ceramic fuel cell of claim 1, wherein, prior to sintering, each of the patterned layer, the anode support layer, and the first electrolyte layer is a green tape.

### Claim 32

A method of making a ceramic fuel cell comprising:
providing a first structure comprising, in order:
a patterned layer comprising, prior to sintering, green bodies having a first composition;
an anode support layer comprising, prior to sintering, green bodies having a second composition; and
a first electrolyte layer comprising, prior to sintering, green bodies having a third composition;
sintering the first structure at a first sintering temperature to obtain a second structure comprising, in order:
a sintered patterned layer;
a sintered anode support layer; and
a sintered first electrolyte layer;
wherein the sintered patterned layer has a first coefficient of thermal expansion, the sintered anode support layer has a second coefficient of thermal expansion, and the sintered first electrolyte layer has a third coefficient of thermal expansion;
the second coefficient of thermal expansion is not between the first coefficient of thermal expansion and the third coefficient of thermal expansion.

### Claim 33 (depends on 32)

The method of claim 32, wherein a thickness of the sintered first electrolyte layer is less than a combined thickness of the sintered patterned layer and the sintered anode support layer.

### Claim 34 (depends on 32)

The method of claim 32, wherein a thickness of the sintered patterned layer is at least as great as a thickness of the sintered first electrolyte layer.

### Claim 35 (depends on 32)

The method of claim 32, wherein a thickness of the sintered patterned layer is 2 to 1500 microns, a thickness of the sintered anode support layer is 250 to 1500 microns, and a thickness of the sintered first electrolyte layer is 2 to 100 microns.

### Claim 36 (depends on 32)

The method of claim 32, wherein a thickness of the sintered first electrolyte layer is between 5 to 30 microns

### Claim 37 (depends on 32)

The method of claim 32, wherein the third coefficient of thermal expansion is within twenty five percent of the first coefficient of thermal expansion.

### Claim 38 (depends on 32)

The method of claim 32, wherein the third coefficient of thermal expansion is within ten percent of the first coefficient of thermal expansion.

### Claim 39 (depends on 32)

The method of claim 32, wherein the third coefficient of thermal expansion is within five percent of the first coefficient of thermal expansion.

### Claim 40 (depends on 32)

The method of claim 32, wherein the third coefficient of thermal expansion is within one percent of the first coefficient of thermal expansion.

### Claim 41 (depends on 32)

The method of claim 32, wherein the first and third coefficients of thermal expansion are substantially the same.

### Claim 42 (depends on 32)

The method of claim 32, wherein the second coefficient of thermal expansion is at least 1 percent different from each of the first and third coefficients of thermal expansion.

### Claim 43 (depends on 32)

The method of claim 32, wherein:
during sintering, the first composition has a first shrinkage, the second composition has a second shrinkage, and the third composition has a third shrinkage; and
the second shrinkage is not between the first shrinkage and the third shrinkage.

### Claim 44 (depends on 43)

The method of claim 43, wherein the third shrinkage is within ten percent of the first shrinkage.

### Claim 45 (depends on 43)

The method of claim 43, wherein the third shrinkage is within three percent of the first shrinkage.

### Claim 46 (depends on 43)

The method of claim 43, wherein the third shrinkage is within one percent of the first shrinkage.

### Claim 47 (depends on 43)

The method of claim 43, wherein the first and third shrinkages are equal.

### Claim 48 (depends on 43)

The method of claim 43, wherein the second shrinkage is at least one percent different from each of the first shrinkage and the third shrinkage.

### Claim 49 (depends on 43)

The method of claim 43, wherein the second shrinkage is between one and ten percent different from each of the first shrinkage and the third shrinkage.

### Claim 50 (depends on 43)

The method of claim 43, wherein the patterned layer, the anode support layer, and the first electrolyte layer are not constrained during sintering.

### Claim 51 (depends on 43)

The method of claim 43, wherein the patterned layer, the anode support layer, and the first electrolyte layer are constrained during sintering

### Claim 52 (depends on 43)

The method of claim 43, further comprising:
after sintering the patterned layer, the anode support layer, and the first electrolyte layer:
providing a second electrolyte layer over the first electrolyte layer, the second electrolyte layer comprising, prior to sintering, green bodies having a fourth composition; and
sintering the second electrolyte layer at a second sintering temperature lower than the first sintering temperature.

### Claim 53 (depends on 43)

The method of claim 43, further comprising:
after sintering the patterned layer, the anode support layer, and the first electrolyte layer:
providing a cathode layer over the first electrolyte layer, the cathode layer comprising, prior to sintering, green bodies having a fifth composition; and
sintering the cathode layer at a second sintering temperature lower than the first sintering temperature.

### Claim 54 (depends on 43)

The method of claim 43, wherein the first composition comprises GDC, the second composition comprises NiO-GDC, and the third composition comprises GDC.

### Claim 55 (depends on 43)

The method of claim 43, wherein the second composition comprises NiO and Ce1-xGdxO2-0.5x powders, and the first and third compositions comprise Ce1-xGdxO2-0.5x powder, wherein 0≦x≦0.2.

### Claim 56 (depends on 43)

The method of claim 43, wherein the first composition and the third composition are at least partially made of the same material.

### Claim 57 (depends on 43)

The method of claim 43, wherein the first composition and the third composition are the same.

### Claim 58 (depends on 43)

The method of claim 43, wherein the first electrolyte layer comprises at least one of yttria stabilized zirconia (YSZ), scandia stabilized zirconia (SSZ), gadolinia doped ceria (GDC), samaria doped ceria (SDC), samarium-neodymium doped ceria (SNDC), strontium and magnesium doped lanthanum gallate (LSGM), and combinations of multiple dopants and stabilizers in these electrolytes.

### Claim 59 (depends on 43)

The method of claim 43, wherein the anode support layer comprises a composite anode comprised of NiO and one or more of yttria stabilized zirconia (YSZ), scandia stabilized zirconia (SSZ), gadolinia doped ceria (GDC), samaria doped ceria (SDC), samarium-neodymium doped ceria (SNDC), strontium and magnesium doped lanthanum gallate (LSGM), and combinations of multiple dopants and stabilizers in these materials.

### Claim 60 (depends on 43)

The method of claim 43, wherein the patterned layer comprises at least one of yttria stabilized zirconia (YSZ), scandia stabilized zirconia (SSZ), gadolinia doped ceria (GDC), samaria doped ceria (SDC), samarium-neodymium doped ceria (SNDC), strontium and magnesium doped lanthanum gallate (LSGM), and combinations of multiple dopants and stabilizers in these materials.

### Claim 61 (depends on 32)

The method of claim 32, wherein the patterned layer comprises one or more apertures.

### Claim 62 (depends on 32)

The method of claim 32, wherein, prior to sintering, each of the patterned layer, the anode support layer, and the first electrolyte layer is a green tape.

### Claim 63

A method of making a ceramic fuel cell comprising:
providing a first structure comprising, in order:
a patterned layer comprising, prior to sintering, green bodies having a first composition;
an anode support layer comprising, prior to sintering, green bodies having a second composition; and
a first electrolyte layer comprising, prior to sintering, green bodies having a third composition;
sintering the first structure at a first sintering temperature to obtain a second structure comprising, in order:
a sintered patterned layer;
a sintered anode support layer; and
a sintered first electrolyte layer;
wherein, during sintering, the first composition has a first shrinkage, the second composition has a second shrinkage, and the third composition has a third shrinkage; and
the second shrinkage is not between the first shrinkage and the third shrinkage.

### Claim 64 (depends on 63)

The method of claim 63, wherein a thickness of the sintered first electrolyte layer is less than a combined thickness of the sintered patterned layer and the sintered anode support layer.

### Claim 65 (depends on 63)

The method of claim 63, wherein a thickness of the sintered patterned layer is at least as great as a thickness of the sintered first electrolyte layer.

### Claim 66 (depends on 63)

The method of claim 63, wherein a thickness of the sintered patterned layer is 2 to 1500 microns, a thickness of the sintered anode support layer is 250 to 1500 microns, and a thickness of the sintered first electrolyte layer is 2 to 100 microns.

### Claim 67 (depends on 63)

The method of claim 63, wherein a thickness of the sintered first electrolyte layer is between 5 to 30 microns.

### Claim 68 (depends on 63)

The method of claim 63, wherein the third shrinkage is within ten percent of the first shrinkage.

### Claim 69 (depends on 63)

The method claim 63, wherein the third shrinkage is within three percent of the first shrinkage.

### Claim 70 (depends on 63)

The method of claim 63, wherein the third shrinkage is within one percent of the first shrinkage.

### Claim 71 (depends on 63)

The method of claim 63, wherein the first and third shrinkages are equal.

### Claim 72 (depends on 63)

The method of claim 63, wherein the second shrinkage is at least one percent different from each of the first shrinkage and the third shrinkage.

### Claim 73 (depends on 63)

The method of claim 63, wherein the second shrinkage is between one and ten percent different from each of the first shrinkage and the third shrinkage.

### Claim 74 (depends on 63)

The method of claim 63, wherein the patterned layer, the anode support layer, and the first electrolyte layer are not constrained during sintering.

### Claim 75 (depends on 63)

The method of claim 63, wherein the patterned layer, the anode support layer, and the first electrolyte layer are constrained during sintering.

### Claim 76 (depends on 63)

The method of claim 63, further comprising:
after sintering the patterned layer, the anode support layer, and the first electrolyte layer:
providing a second electrolyte layer over the first electrolyte layer, the second electrolyte layer comprising, prior to sintering, green bodies having a fourth composition; and
sintering the second electrolyte layer at a second sintering temperature lower than the first sintering temperature.

### Claim 77 (depends on 63)

The method of claim 63, further comprising:
after sintering the patterned layer, the anode support layer, and the first electrolyte layer:
providing a cathode layer over the first electrolyte layer, the cathode layer comprising, prior to sintering, green bodies having a fifth composition; and
sintering the cathode layer at a second sintering temperature lower than the first sintering temperature.

### Claim 78 (depends on 63)

The method of claim 63, wherein the sintered patterned layer has a first coefficient of thermal expansion, the sintered anode support layer has a second coefficient of thermal expansion, and the sintered first electrolyte layer has a third coefficient of thermal expansion, and wherein the second coefficient of thermal expansion is not between the first coefficient of thermal expansion and the third coefficient of thermal expansion.

### Claim 79 (depends on 78)

The method of claim 78, wherein the third coefficient of thermal expansion is within twenty five percent of the first coefficient of thermal expansion.

### Claim 80 (depends on 78)

The method of claim 78, wherein the third coefficient of thermal expansion is within ten percent of the first coefficient of thermal expansion.

### Claim 81 (depends on 78)

The method of claim 78, wherein the third coefficient of thermal expansion is within five percent of the first coefficient of thermal expansion.

### Claim 82 (depends on 78)

The method of claim 78, wherein the third coefficient of thermal expansion is within one percent of the first coefficient of thermal expansion.

### Claim 83 (depends on 78)

The method of claim 78, wherein first and third coefficients of thermal expansion are substantially the same.

### Claim 84 (depends on 78)

The method of claim 78, wherein the second coefficient of thermal expansion is at least 1 percent different from each of the first and third coefficients of thermal expansion.

### Claim 85 (depends on 63)

The method of claim 63, wherein the first composition comprises GDC, the second composition comprises NiO-GDC, and the third composition comprises GDC.

### Claim 86 (depends on 63)

The method of claim 63, wherein the second composition comprises NiO and Ce1-xGdxO2-0.5x powders, and the first and third compositions comprise Ce1-xGdxO2-0.5x powder, wherein 0≦x≦0.2.

### Claim 87 (depends on 63)

The method of claim 63, wherein the first composition and the third composition are at least partially made of the same material.

### Claim 88 (depends on 63)

The method of claim 63, wherein the first composition and the third composition are the same.

### Claim 89 (depends on 63)

The method of claim 63, wherein the first electrolyte layer comprises at least one of yttria stabilized zirconia (YSZ), scandia stabilized zirconia (SSZ), gadolinia doped ceria (GDC), samaria doped ceria (SDC), samarium-neodymium doped ceria (SNDC), strontium and magnesium doped lanthanum gallate (LSGM), and combinations of multiple dopants and stabilizers in these electrolytes.

### Claim 90 (depends on 63)

The method of claim 63, wherein the anode support layer comprises a composite anode comprised of NiO and one or more of yttria stabilized zirconia (YSZ), scandia stabilized zirconia (SSZ), gadolinia doped ceria (GDC), samaria doped ceria (SDC), samarium-neodymium doped ceria (SNDC), strontium and magnesium doped lanthanum gallate (LSGM), and combinations of multiple dopants and stabilizers in these materials.

### Claim 91 (depends on 63)

The method of claim 63, wherein the patterned layer comprises at least one of yttria stabilized zirconia (YSZ), scandia stabilized zirconia (SSZ), gadolinia doped ceria (GDC), samaria doped ceria (SDC), samarium-neodymium doped ceria (SNDC), strontium and magnesium doped lanthanum gallate (LSGM), and combinations of multiple dopants and stabilizers in these materials.

### Claim 92 (depends on 63)

The method of claim 63, wherein the patterned layer comprises one or more apertures.

### Claim 93 (depends on 63)

The method of claim 63, wherein, prior to sintering, each of the patterned layer, the anode support layer, and the first electrolyte layer is a green tape.

### Claim 94

A ceramic fuel cell comprising:
a second structure comprising, in order:
a sintered patterned layer;
a sintered anode support layer; and
a sintered first electrolyte layer;
wherein the second structure is obtained by the process of:
providing a first structure comprising, in order:
a patterned layer comprising, prior to sintering, green bodies having a first composition;
an anode support layer comprising, prior to sintering, green bodies having a second composition; and
a first electrolyte layer comprising, prior to sintering, green bodies having a third composition;
sintering the first structure at a first sintering temperature;
wherein, during sintering, the first composition has a first shrinkage, the second composition has a second shrinkage, and the third composition has a third shrinkage; and
the second shrinkage is not between the first shrinkage and the third shrinkage.

### Claim 95 (depends on 94)

The ceramic fuel cell of claim 94, wherein a thickness of the sintered first electrolyte layer is less than a combined thickness of the sintered patterned layer and the sintered anode support layer.

### Claim 96 (depends on 94)

The ceramic fuel cell of claim 94, wherein a thickness of the sintered patterned layer is at least as great as a thickness of the sintered first electrolyte layer.

### Claim 97 (depends on 94)

The ceramic fuel cell of claim 94, wherein a thickness of the sintered patterned layer is 2 to 1500 microns, a thickness of the sintered anode support layer is 250 to 1500 microns, and a thickness of the sintered first electrolyte layer is 2 to 100 microns.

### Claim 98 (depends on 94)

The ceramic fuel cell of claim 94, wherein a thickness of the sintered first electrolyte layer is between 5 to 30 microns.

### Claim 99 (depends on 94)

The ceramic fuel cell of claim 94, wherein the third shrinkage is within ten percent of the first shrinkage.

### Claim 100 (depends on 94)

The ceramic fuel cell of claim 94, wherein the third shrinkage is within three percent of the first shrinkage.

### Claim 101 (depends on 94)

The ceramic fuel cell of claim 94, wherein the third shrinkage is within one percent of the first shrinkage.

### Claim 102 (depends on 94)

The ceramic fuel cell of claim 94, wherein the first and third shrinkages are equal.

### Claim 103 (depends on 94)

The ceramic fuel cell of claim 94, wherein the second shrinkage is at least one percent different from each of the first shrinkage and the third shrinkage.

### Claim 104 (depends on 94)

The ceramic fuel cell of claim 94, wherein the second shrinkage is between one and ten percent different from each of the first shrinkage and the third shrinkage.

### Claim 105 (depends on 94)

The ceramic fuel cell of claim 94, wherein the patterned layer, the anode support layer, and the first electrolyte layer are not constrained during sintering.

### Claim 106 (depends on 94)

The ceramic fuel cell of claim 94, wherein the patterned layer, the anode support layer, and the first electrolyte layer are constrained during sintering.

### Claim 107 (depends on 94)

The ceramic fuel cell of claim 94, further comprising:
after sintering the patterned layer, the anode support layer, and the first electrolyte layer:
providing a second electrolyte layer over the first electrolyte layer, the second electrolyte layer comprising, prior to sintering, green bodies having a fourth composition; and
sintering the second electrolyte layer at a second sintering temperature lower than the first sintering temperature.

### Claim 108 (depends on 94)

The ceramic fuel cell of claim 94, further comprising:
after sintering the patterned layer, the anode support layer, and the first electrolyte layer:
providing a cathode layer over the first electrolyte layer, the cathode layer comprising, prior to sintering, green bodies having a fifth composition; and
sintering the cathode layer at a second sintering temperature lower than the first sintering temperature.

### Claim 109 (depends on 94)

The ceramic fuel cell of claim 94, wherein the sintered patterned layer has a first coefficient of thermal expansion, the sintered anode support layer has a second coefficient of thermal expansion, and the sintered first electrolyte layer has a third coefficient of thermal expansion, and wherein the second coefficient of thermal expansion is not between the first coefficient of thermal expansion and the third coefficient of thermal expansion.

### Claim 110 (depends on 109)

The ceramic fuel cell of claim 109, wherein the third coefficient of thermal expansion is within twenty five percent of the first coefficient of thermal expansion.

### Claim 111 (depends on 109)

The ceramic fuel cell of claim 109, wherein the third coefficient of thermal expansion is within ten percent of the first coefficient of thermal expansion.

### Claim 112 (depends on 109)

The ceramic fuel cell of claim 109, wherein the third coefficient of thermal expansion is within five percent of the first coefficient of thermal expansion.

### Claim 113 (depends on 109)

The ceramic fuel cell of claim 109, wherein the third coefficient of thermal expansion is within one percent of the first coefficient of thermal expansion.

### Claim 114 (depends on 109)

The ceramic fuel cell of claim 109, wherein the first and third coefficients of thermal expansion are substantially the same.

### Claim 115 (depends on 109)

The ceramic fuel cell of claim 109, wherein the second coefficient of thermal expansion is at least 1 percent different from each of the first and third coefficients of thermal expansion.

### Claim 116 (depends on 94)

The ceramic fuel cell of claim 94, wherein the first composition comprises GDC, the second composition comprises NiO-GDC, and the third composition comprises GDC.

### Claim 117 (depends on 94)

The ceramic fuel cell of claim 94, wherein the second composition comprises NiO and Ce1-xGdxO2-0.5x powders, and the first and third compositions comprise Ce1-xGdxO2-0.5x powder, wherein 0≦x≦0.2.

### Claim 118 (depends on 94)

The ceramic fuel cell of claim 94, wherein the first composition and the third composition are at least partially made of the same material.

### Claim 119 (depends on 94)

The ceramic fuel cell of claim 94, wherein the first composition and the third composition are the same.

### Claim 120 (depends on 94)

The ceramic fuel cell of claim 94, wherein the first electrolyte layer comprises at least one of yttria stabilized zirconia (YSZ), scandia stabilized zirconia (SSZ), gadolinia doped ceria (GDC), samaria doped ceria (SDC), samarium-neodymium doped ceria (SNDC), strontium and magnesium doped lanthanum gallate (LSGM), and combinations of multiple dopants and stabilizers in these electrolytes.

### Claim 121 (depends on 94)

The ceramic fuel cell of claim 94, wherein the anode support layer comprises a composite anode comprised of NiO and one or more of yttria stabilized zirconia (YSZ), scandia stabilized zirconia (SSZ), gadolinia doped ceria (GDC), samaria doped ceria (SDC), samarium-neodymium doped ceria (SNDC), strontium and magnesium doped lanthanum gallate (LSGM), and combinations of multiple dopants and stabilizers in these materials.

### Claim 122 (depends on 94)

The ceramic fuel cell of claim 94, wherein the patterned layer comprises at least one of yttria stabilized zirconia (YSZ), scandia stabilized zirconia (SSZ), gadolinia doped ceria (GDC), samaria doped ceria (SDC), samarium-neodymium doped ceria (SNDC), strontium and magnesium doped lanthanum gallate (LSGM), and combinations of multiple dopants and stabilizers in these materials.

### Claim 123 (depends on 94)

The ceramic fuel cell of claim 94, wherein the patterned layer comprises one or more apertures.

### Claim 124 (depends on 94)

The ceramic fuel cell of claim 94, wherein, prior to sintering, each of the patterned layer, the anode support layer, and the first electrolyte layer is a green tape.