# US 2014/0209214 A1 · Method and steel component

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2014/0209214 A1
- Document ID: US20140209214A1
- Status: Published application
- Kind: A1
- Application number: 14/122,215
- Filed: 2012-05-22
- Published: 2014-07-31
- Earliest claimed: 2011-05-25
- Assignees: Aktiebolaget Skf
- Applicants: Aktiebolaget Skf
- Inventors: Thore Lund
- Web page: https://patentgrep.com/patent/US20140209214A1

## CPC

- C23C 8/80: After-treatment
- C21D 1/20: Isothermal quenching, e.g. bainitic hardening
- C21D 9/36: for balls; for rollers
- C21D 9/40: for rings; for bearing races
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/22: with molybdenum or tungsten
- C22C 38/24: with vanadium
- C23C 8/32: of ferrous surfaces
- F16C 33/32: Balls
- F16C 33/64: Special methods of manufacture
- C21D 1/18: Hardening (C21D1/02 takes precedence); Quenching with or without subsequent tempering (quenching devices C21D1/62)
- C21D 2211/002: Bainite
- C21D 2221/10: Differential treatment of inner with respect to outer regions, e.g. core and periphery, respectively
- F16C 2360/31: Wind motors
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- F16C: SHAFTS; FLEXIBLE SHAFTS; ELEMENTS OR CRANKSHAFT MECHANISMS; ROTARY BODIES OTHER THAN GEARING ELEMENTS; BEARINGS

## Abstract

Method for heat treating a steel component (28, 36) comprising the steps of: a) carbonitriding the steel component (28, 36) at a temperature of 930-970° C., b) cooling the steel component (28, 36), d) re-heating the steel component (28, 36) to a temperature of 780-820° C. and d) quenching the steel component (28, 36). The method comprises the step of either e) performing a bainite transformation at a temperature just above the martensite formation temperature, transforming 25-99% of the austenite into bainite at the temperature and then increasing the temperature to speed up the transformation of the remaining austenite into bainite, or f) holding the steel component (28, 36) at an initial temperature (T1) above the initial martensite formation temperature (Ms), and lowering the initial temperature (T1) to a temperature (T2) that is below the initial martensite formation temperature (Ms) but above the actual martensite formation temperature during the bainite transformation.

## Claims

### Claim 1

A method for heat treating a steel component comprising the steps of:
a) carbonitriding the steel component at a temperature of 930-970° C.
b) cooling the steel component,
c) re-heating the steel component to a temperature of 780-820° C. and
d) quenching the steel component, wherein the method further comprises one of the following steps
e) performing a bainite transformation at a temperature above the martensite formation temperature, transforming 25-99% of the austenite into bainite at that temperature and then increasing the temperature to speed up the transformation of the remaining austenite into bainite, or
f) holding the steel component at an initial temperature (T1) above the initial martensite formation temperature (Ms), and lowering the initial temperature (T1) to a temperature (T2) that is below the initial martensite formation temperature (Ms) but above the actual martensite formation temperature during the bainite transformation.

### Claim 2 (depends on 1)

The method according to claim 1, wherein step e) further comprises transforming 50-90% of the austenite to bainite before increasing the temperature for speeding up the transformation of the remaining austenite into bainite.

### Claim 3 (depends on 1)

The method according to claim 1, wherein step f) further comprises subsequently raising the temperature from (T2) to a temperature (T3) that is above the initial martensite formation temperature (Ms) during the bainite transformation.

### Claim 4 (depends on 3)

The method according to claim 3, wherein step f) further comprises the step of transforming at least 15-40% of the austenite into bainite at a temperature (T1) above the initial martensite formation temperature (Ms) before lowering the temperature (T1) to a temperature (T2) below the initial martensite formation temperature (Ms) but above the actual martensite formation temperature.

### Claim 5 (depends on 3)

The method according to claim 3, wherein step f) further comprises the step of maintaining the temperature (T3) above the initial martensite formation temperature (Ms) until complete bainite transformation is achieved.

### Claim 6 (depends on 5)

The method according to claim 5 wherein step a) further comprises carbonitriding the steel component at a temperature of 930-970° C. for 5-10 hours.

### Claim 7 (depends on 6)

The method according to claim 6, wherein the steel component further comprises steel with a carbon content of 0.6 to 1.20 weight %.

### Claim 8 (depends on 6)

The method according to claim 6, wherein the steel component further comprises steel with a carbon content of 0.2 to 0.6 weight %.

### Claim 9 (depends on 8)

The method according to claim 8, wherein the steel comprises, by weight, max 20 ppm S and max 15 ppm O and includes sulphide inclusions and less than 5% of the sulphide inclusions contain encapsulated or embedded oxide inclusions.

### Claim 10 (depends on 9)

The method according to claim 9, wherein the maximum length of the sulphide inclusions is 125 mm at a Reduced Variate equal to 3.

### Claim 11 (depends on 10)

The method according to claim 10, wherein the steel comprises max 10 ppm O or max 8 ppm O.

### Claim 12 (depends on 10)

The method according to claim 10, wherein all of the sulphide inclusions have an aspect ratio less than 3:1.

### Claim 13 (depends on 12)

The method according to claim 12, wherein the steel comprises an element selected from the group: Ca, Mg, Te, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb or Lu.

### Claim 14 (depends on 13)

The method according to claim 13, wherein the steel comprises, by weight, 10-30 ppm of said element.

### Claim 15 (depends on 14)

The method according to claim 14, wherein the steel component constitutes at least part of one of the following: a ball bearing, a roller bearing, a needle bearing, a tapered roller bearing, a spherical roller bearing, a toroidal roller bearing, a ball thrust bearing, a roller thrust bearing, a tapered roller thrust bearing, a wheel bearing, a hub bearing unit, a slewing bearing, a ball screw, and a component for an application in which it is subjected to alternating Hertzian stresses, such as rolling contact or combined rolling and sliding and/or an application that requires high wear resistance and/or increased fatigue and tensile strength.

### Claim 16 (depends on 15)

The method according to claim 15, wherein the steel component is provided with a carbonitrided layer having a thickness (d) of 0.3-1.2 mm whereby all of the carbides in the carbonitrided layer have a maximum longitudinal dimension of 0.2-0.3 mm.

### Claim 17 (depends on 16)

The method according to claim 16, wherein the steel component is provided with a carbonitrided layer having a ratio (d:D) of depth (d) of the carbonitrided layer measured from the surface of the steel component to maximum transverse dimension (D) of the steel component of 1:4000 to 1:17,000 or more.

### Claim 18

The method according to clam 17, wherein the steel component has a substantially bainitic structure and a hardness of at least 62 HRC.

### Claim 19

(canceled)

### Claim 20

(canceled)

### Claim 21 (depends on 1)

The method according to claim 1, wherein the steel component is used in a wind turbine application.