# US 2014/0194603 A1 · Method for the production of lignin-containing precursor fibres and also carbon fibres

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2014/0194603 A1
- Document ID: US20140194603A1
- Status: Published application
- Kind: A1
- Application number: 14/118,149
- Filed: 2012-05-16
- Published: 2014-07-10
- Earliest claimed: 2011-05-18
- Assignees: Stora Enso OYJ
- Inventors: Andre Lehmann; Horst Ebeling; Hans-Peter Fink
- Web page: https://patentgrep.com/patent/US20140194603A1

## CPC

- D01F 9/17: from lignin
- B29C 48/05: Filamentary, e.g. strands
- B29D 99/0078: {Producing filamentary materials}
- C08L 97/02: Lignocellulosic material, e.g. wood, straw or bagasse {(manufacture of articles made from lignocellulosic material by dry processes B27N)}
- D01D 5/06: Wet spinning methods {(D01D5/0046 takes precedence)}
- D01F 9/00: Artificial filaments or the like of other substances; Manufacture thereof; Apparatus specially adapted for the manufacture of carbon filaments
- B29K 2033/20: PAN, i.e. polyacrylonitrile
- B29L 2031/731: {Filamentary material, i.e. comprised of a single element, e.g. filaments, strands, threads, fibres (cables B29L2031/707)}
- D01F: CHEMICAL FEATURES IN THE MANUFACTURE OF ARTIFICIAL FILAMENTS, THREADS, FIBRES, BRISTLES OR RIBBONS; APPARATUS SPECIALLY ADAPTED FOR THE MANUFACTURE OF CARBON FILAMENTS
- B29C: SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING (making preforms B29B11/00; making laminated products by combining previously unconnected layers which become one product whose layers will remain together B32B37/00 - B32B41/00)
- B29D: PRODUCING PARTICULAR ARTICLES FROM PLASTICS OR FROM SUBSTANCES IN A PLASTIC STATE (making granules B29B9/00; making preforms B29B11/00)
- C08L: COMPOSITIONS OF MACROMOLECULAR COMPOUNDS (compositions based on polymerisable monomers C08F, C08G; artificial filaments or fibres D01F; textile treating compositions D06)
- D01D: MECHANICAL METHODS OR APPARATUS IN THE MANUFACTURE OF ARTIFICIAL FILAMENTS, THREADS, FIBRES, BRISTLES OR RIBBONS
- B29K: INDEXING SCHEME ASSOCIATED WITH SUBCLASSES B29B, B29C OR B29D, RELATING TO MOULDING MATERIALS OR TO MATERIALS FOR {MOULDS, } REINFORCEMENTS, FILLERS OR PREFORMED PARTS, e.g. INSERTS
- B29L: INDEXING SCHEME ASSOCIATED WITH SUBCLASS B29C, RELATING TO PARTICULAR ARTICLES

## Abstract

The invention relates to a method for the production of a precursor for the production of carbon- and activated carbon fibres according to the wet- or air-gap spinning method, in which a solution of lignin and a fibre-forming polymer in a suitable solvent is extruded through the holes of a spinning nozzle into a coagulation bath, the formed thread is stretched and subsequently treated, dried at an elevated temperature and then wound up. The lignin-containing thread is an economical starting material for the production of carbon- and activated carbon fibres.

## Claims

### Claim 1

A method for the production of a lignin-containing precursor fibre for the production of carbon fibres and/or activated carbon fibres, comprising
a) forming a solution, comprising at least one sort of lignin and also at least one fibre-forming polymer selected from the group consisting of cellulose or cellulose derivatives in at least one solvent, selected from the group consisting of tertiary amine oxides, ionic liquids, aprotic polar solvents, dimethylformamide and dimethylacetamide, and mixtures thereof, and
b) transferring the solution into a coagulation bath by extruding the solution through a spinning nozzle by a wet spinning or an air-gap spinning method, the lignin-containing precursor fibre precipitating.

### Claim 2 (depends on 1)

The method according to claim 1, wherein the solution formed in step a) is produced by agitation or kneading of the at least one sort of lignin and also of the at least one fibre-forming polymer in the at least one solvent, at temperatures of 60° C. or more.

### Claim 3 (depends on 1)

The method according claim 1, wherein the solution is filtered before introduction into the coagulation bath.

### Claim 4 (depends on 1)

The method according to claim 1 wherein the spinning nozzle has a spinning hole diameter from 50 to 600 pm.

### Claim 5 (depends on 4)

The method according to claim 4 wherein the transferring step is performed by the wet spinning or the air-gap spinning method, wherein there is an air gap of at least 10 mm and at most 500 mm.

### Claim 6 (depends on 1)

The method according to claim 1 wherein the lignin-containing precursor fibre
a) is stretched to at least 1.1 times its length, at a temperature of at least 60° C., the stretching being implemented preferably in the precipitation bath, in air or in water vapour,
b) is washed with demineralised water,
c) is treated subsequently with textile aids for improving the thread strength and for avoiding electrostatic charges,
d) is dried by winding up or winding round of the fibre onto or around heated rollers or by through-flow drying at a temperature of at least 80° C., and
e) is wound up.

### Claim 7 (depends on 6)

The method according to claim 6 wherein the fibre is treated with a spinning oil before drying, after drying or before and after drying.

### Claim 8 (depends on 1)

The method according to claim 1 wherein respectively relative to the entire solution,
a) the at least one sort of lignin has a concentration from 2 to 30% by weight, and
b) the at least one fibre-forming polymer has a concentration from 5 to 40% by weight.

### Claim 9 (depends on 1)

The method according to claim 1 wherein the coagulation bath comprises water or a mixture of water and an organic liquid selected from the group consisting of aprotic polar solvents, aliphatic amides which are liquid at room temperature, tertiary amine oxides, and ionic liquids.

### Claim 10 (depends on 9)

The method according to claim 9 wherein the pH value of the coagulation bath is between 1 and 7.

### Claim 11 (depends on 1)

The method according to claim 1 wherein the aprotic polar solvent is dimethylsulfoxid (DMSO) and the tertiary amine oxide is aqueous N-methylmorpholine-N-oxide (NMMO), and the ionic liquids are selected from the group consisting of imidazolium compounds, pyridinium compounds and tetraalkylammonium compounds, and mixtures thereof.

### Claim 12 (depends on 1)

The method according to claim 1 wherein the cellulose or cellulose derivatives, are selected of the group consisting of cellulose carbamate, cellulose allophanate, hemicelluloses, and mixtures thereof.

### Claim 13 (depends on 1)

The method according to claim 1 wherein the at least one sort of lignin results from wood and annual plant pulping methods and is selected from the group consisting of alkali lignin, kraft lignin, lignosulphonate, thiolignin, organosolvlignin, ASAM lignin, lignins from digestion processes by means of ionic liquids or enzymes and combinations thereof.

### Claim 14

A precursor fibre for the production of carbon fibres, comprising:
a) a content of at least one sort of lignin of 1% to 99% weight,
b) a content of at least one sort of fibre-forming polymer of 1 to 99% by weight, and
c) a strength of at least 10 cN/tex, or
a modulus of elasticity of at least 1,000 cN/tex.

### Claim 15 (depends on 1)

The precursor fibre, produced according to a method according to one of the claim 1.

### Claim 16 (depends on 14)

A method for the production of a carbon fibre in which a precursor fibre according to claim 14 is stabilised at temperatures between 100 and 600° C. and is carbonised above 800° C. under inert conditions.

### Claim 17 (depends on 16)

The method according to claim 16 wherein the carbon fibre is subjected to water vapour, after the carbonisation, at temperatures greater than 200° C.

### Claim 18 (depends on 1)

A carbon fibre, producible according to a method of claim 1.

### Claim 19 (depends on 2)

The method according to claim 2 wherein the temperature is above 80° C.

### Claim 20 (depends on 4)

The method according to claim 4 wherein the spinning hole diameter of the spinning nozzle is between 100 and 500 pm.

### Claim 21 (depends on 5)

The method according to claim 5 wherein the air gap is at least 20 mm.

### Claim 22 (depends on 6)

The method according to claim 6 wherein the lignin-containing fibre is stretched to at most 12 times.

### Claim 23 (depends on 6)

The method according to claim 6 wherein the lignin-containing fibre is stretched to at least 1.5 times.

### Claim 24 (depends on 6)

The method according to claim 6 wherein the lignin-containing fibre is stretched at a temperature of at least 80° C.

### Claim 25 (depends on 6)

The method according to claim 6 wherein the lignin-containing fibre is stretched at a temperature of at least 100° C.

### Claim 26 (depends on 6)

The method according to claim 6 wherein the lignin-containing fibre is dried at a temperature of at least 100° C.

### Claim 27 (depends on 8)

The method according to claim 8, where the concentration of the at least one sort of lignin is between 3 and 20% by weight.

### Claim 27 (depends on 9)

The method according to claim 9 wherein the ionic liquids are selected from the group consisting of 1 -butyl-3-methylimidazolium chloride, 1-butyl-3-methylimidazolium acetate, and 1-ethyl-3-methylimidazolium acetate.

### Claim 28 (depends on 8)

The method according to claim 8 wherein the concentration of the at least one fibre-forming polymer is between 7 and 30% by weight.

### Claim 28 (depends on 10)

The method according to claim 10, wherein the pH value of the coagulation bath is between 2 and 5.

### Claim 29 (depends on 14)

The precursor fibre according to claim 14 wherein the fibre has a strength of at least 20 cN/tex and a modulus of elasticity of at least 1,300 cN/tex,

### Claim 30 (depends on 17)

The method according to claim 17, wherein the carbon fibre is subjected to water vapour, after the carbonisation, at temperatures greater than 300° C.