# US 2014/0154177 A1 · Metallophosphate molecular sieves, method of preparation and use

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2014/0154177 A1
- Document ID: US20140154177A1
- Status: Published application
- Kind: A1
- Application number: 13/690,087
- Filed: 2012-11-30
- Published: 2014-06-05
- Earliest claimed: 2012-11-30
- Assignees: Uop LLC
- Applicants: Uop LLC
- Inventors: Gregory J. Lewis; Lisa M. Knight; Paulina Jakubczak; Justin E. Stanczyk
- Web page: https://patentgrep.com/patent/US20140154177A1

## CPC

- C01B 39/54: Phosphates, e.g. APO or SAPO compounds
- C01B 37/04: Aluminophosphates [APO compounds]
- C01B 37/065: {the other elements being metals only}
- C01B 37/08: Silicoaluminophosphates [SAPO compounds] {, e.g. CoSAPO}
- C07F 19/00: Metal compounds according to more than one of main groups C07F1/00 - C07F17/00
- C01B: NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; {METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C}
- C07F: ACYCLIC, CARBOCYCLIC OR HETEROCYCLIC COMPOUNDS CONTAINING ELEMENTS OTHER THAN CARBON, HYDROGEN, HALOGEN, OXYGEN, NITROGEN, SULFUR, SELENIUM OR TELLURIUM (metal-containing porphyrins C07D487/22)

## Abstract

A new family of crystalline microporous metallophosphates designated AlPO-67 has been synthesized. These metallophosphates are represented by the empirical formula R+rMm2+EPxSiyOz where R is an organoammonium cation such as the ETMA+ or DEDMA+, M is a framework metal alkaline earth or transition metal of valence 2+, and E is a trivalent framework element such as aluminum or gallium. The AlPO-67 compositions exhibit the LEV framework topology and have catalytic properties for carrying out various hydrocarbon conversion processes and separation properties for separating at least one component.

## Claims

### Claim 1

A microporous crystalline metallophosphate material having a three-dimensional framework of EO2− and PO2+ and at least one of [M2+O2]2− and SiO2 tetrahedral units and an empirical composition in the as synthesized and anhydrous basis expressed by an empirical formula of:
RrM2+mEPxSiyOz
where M is at least one framework cation of +2 valence selected from the group consisting of alkaline earth and transition metals, “m” is the mole ratio of M to E and varies from 0 to about 1.0, R is an organoammonium cation selected from the group consisting of ethyltrimethylammonium (ETMA+), diethyldimethylammonium (DEDMA+), and mixtures thereof, “r” is the mole ratio of R to E and has a value of about 0.1 to about 2, E is a trivalent element selected from the group consisting of aluminum, gallium, iron, boron and mixtures thereof, “x” is the mole ratio of P to E and has a value of 0.5 to about 2.0, “y” is the mole ratio of Si to E and varies from 0 to about 1.0, “m”+“y”≧0.02, and “z” is the mole ratio of 0 to (Al+E) and has a value determined by the equation:
z=(2·m+r+3+5·x+4·y)/2
and is characterized in that it has the x-ray diffraction pattern having at least the d-spacings and intensities set forth in Table A1:
TABLE A1
2Θ
d(Å)
I/I0%
8.86-8.39
9.97-10.53
w-m
11.21-10.51
7.89-8.41
m-s
13.65-13.16
6.48-6.72
m-vs
17.72-16.91
5.00-5.24
m-vs
21.29-20.69
4.17-4.29
m-s
22.43-21.5
3.96-4.13
s-vs
23.84-22.84
3.73-3.89
w-vs
27.51-26.51
3.24-3.36
w-m
29.06-27.95
3.07-3.19
w-m
32.90-31.59
2.72-2.83
m
35.02-33.93
2.56-2.64
w-m
36.65-35.31
2.45-2.54
w-m
52.23-50.67
1.75-1.80
w-m

### Claim 2 (depends on 1)

The metallophosphate material of claim 1 where M is selected from the group consisting of beryllium, magnesium, zinc, cobalt, manganese, iron(II), nickel and mixtures thereof.

### Claim 3 (depends on 1)

The metallophosphate material of claim 1 where E is aluminum.

### Claim 4 (depends on 1)

The metallophosphate material of claim 1 where “y” is zero.

### Claim 5 (depends on 1)

The metallophosphate material of claim 1 where “m” is zero.

### Claim 6 (depends on 1)

The metallophosphate material of claim 1 where “m” and “y” are each greater than zero and “m”+“y”≧0.02.

### Claim 7 (depends on 1)

The metallophosphate material of claim 1 where the metallophosphate material is thermally stable up to a temperature of at least 400° C.

### Claim 8 (depends on 1)

The metallophosphate material of claim 1 where the metallophosphate material is thermally stable up to a temperature of at least 500° C.

### Claim 9 (depends on 1)

The metallophosphate material of claim 1 where R is ETMA+.

### Claim 10 (depends on 1)

The metallophosphate material of claim 1 where R is DEDMA+.

### Claim 11 (depends on 1)

The metallophosphate material of claim 1 where R is a mixture of ETMA+ and DEDMA+.

### Claim 12

A process for preparing a microporous crystalline metallophosphate having a three-dimensional framework of EO2−, PO2+ and at least one of [M2+O2]2− and SiO2 tetrahedral units and a composition in the as synthesized and anhydrous basis expressed by an empirical formula of:
RrMm2+EPxSiyOz
where M is at least one framework cation of valence 2+ selected from the group consisting of alkaline earth and transition metals, “m” is the mole ratio of M to E and varies from 0 to about 1.0, R is an organoammonium cation selected from the group consisting of ethyltrimethylammonium (ETMA+), diethyldimethylammonium (DEDMA+), and mixtures thereof, “r” is the mole ratio of R to E and has a value of about 0.1 to about 2.0, E is a trivalent element selected from the group consisting of aluminum, gallium, iron(III), boron and mixtures thereof, “x” is the mole ratio of P to E and varies from 0.5 to about 2.0, “y” is the mole ratio of Si to E and varies from 0 to about 1.0, “m”+“y”≧0.02, and “z” is the mole ratio of 0 to E and has a value determined by the equation:
z=(2·m+r+3+5·x+4·y)/2
and is characterized in that it has the x-ray diffraction pattern having at least the d-spacings and intensities set forth in Table A1:
TABLE A1
2Θ
d(Å)
I/I0%
8.86-8.39
9.97-10.53
w-m
11.21-10.51
7.89-8.41
m-s
13.65-13.16
6.48-6.72
m-vs
17.72-16.91
5.00-5.24
m-vs
21.29-20.69
4.17-4.29
m-s
22.43-21.5
3.96-4.13
s-vs
23.84-22.84
3.73-3.89
w-vs
27.51-26.51
3.24-3.36
w-m
29.06-27.95
3.07-3.19
w-m
32.90-31.59
2.72-2.83
m
35.02-33.93
2.56-2.64
w-m
36.65-35.31
2.45-2.54
w-m
52.23-50.67
1.75-1.80
w-m
the process comprising forming a reaction mixture containing reactive sources of R, E, P, at least one of M and Si, and heating the reaction mixture at a temperature of about 60° C. to about 200° C., for a time sufficient to form the metallophosphate, the reaction mixture having a composition expressed in terms of mole ratios of the oxides of:
aR2O:bMO:E2O3:cP2O5:dSiO2:eH2O
where “a” has a value of about 0.25 to about 16, “b” has a value of about 0 to about 2.0, “c” has a value of about 0.8 to about 8, “d” has a value of about 0 to about 4, and “e” has a value of about 30 to 800 and wherein the sum of the values of “b” and “d” is greater than 0.01.

### Claim 13 (depends on 12)

The process of claim 12 where M is selected from the group consisting of beryllium, magnesium, zinc, cobalt, manganese, nickel, iron (II) and mixtures thereof.

### Claim 14 (depends on 12)

The process of claim 12 where the source of M is selected from the group consisting of halide salts, nitrate salts, acetate salts, sulfate salts and mixtures thereof.

### Claim 15 (depends on 12)

The process of claim 12 where the source of E is selected from the group consisting of aluminum isopropoxide, aluminum sec-butoxide, precipitated alumina, Al(OH)3, aluminum metal, aluminum salts, boric acid, precipitated gallium oxyhydroxide, gallium sulfate, ferric sulfate, ferric chloride and mixtures thereof.

### Claim 16 (depends on 12)

The process of claim 12 where the silicon source is selected from the group consisting of tetraethyorthosilicate, fumed silica, colloidal silica and precipitated silica.

### Claim 17 (depends on 12)

The process of claim 12 where the reaction mixture is reacted at a temperature of about 125° C. to about 175° C. for a time of about 1 day to about 10 days.

### Claim 18 (depends on 12)

The process of claim 12 where R is ETMA+.

### Claim 19 (depends on 12)

The process of claim 12 where R is DEDMA+.

### Claim 20 (depends on 12)

The process of claim 12 where R is a combination of ETMA+ and DEDMA+.

### Claim 21 (depends on 12)

The process of claim 12 further comprising adding AlPO-67 seeds to the reaction mixture.

### Claim 22 (depends on 1)

A modified form of the metallophosphate of claim 1, said modification comprising ammonia calcination under ammonia calcinations conditions, and optionally an additional ion-exchange to form a modified microporous metallophosphate, AlPO-67M, having a three-dimensional framework of EO2−, PO2+ and at least one of [M2+O2]2− and SiO2 tetrahedral units the composition given by the empirical formula:
M′np+Mm2+EPxSiyOz
where M is at least one metal cation of valence +2 selected from the group consisting of Be2+, Mg2+, Zn2+, Co2+, Mn2+, Fe2+, Ni2+, “m” is the mole ratio of M to E and varies from 0 to about 1.0, M′ is selected from the group consisting of NH4+, H+, alkali metals, alkaline earth metals, rare earth metals and mixtures thereof, “n” is the mole ratio of M′ to E and has a value of about 0.03 to about 2.0, “p” is the weighted average valence of M′ and varies from 1 to about 3, E is an trivalent element selected from the group consisting of aluminum, gallium, iron, boron and mixtures thereof, “x” is mole ratio of P to E and varies from 0.5 to about 2.0, “y” is the mole ratio of Si to E and varies from 0 to about 1.0, “m”+“y”≧0.02, and “z” is the mole ratio of O to E and has a value determined by the equation:
z=(p·n+2·m+3+5·x+4·y)/2
and is characterized in that it has the x-ray diffraction pattern having at least the d-spacings and intensities set forth in Table A1:
TABLE A1
2Θ
d(Å)
I/I0%
8.86-8.39
9.97-10.53
w-m
11.21-10.51
7.89-8.41
m-s
13.65-13.16
6.48-6.72
m-vs
17.72-16.91
5.00-5.24
m-vs
21.29-20.69
4.17-4.29
m-s
22.43-21.5
3.96-4.13
s-vs
23.84-22.84
3.73-3.89
w-vs
27.51-26.51
3.24-3.36
w-m
29.06-27.95
3.07-3.19
w-m
32.90-31.59
2.72-2.83
m
35.02-33.93
2.56-2.64
w-m
36.65-35.31
2.45-2.54
w-m
52.23-50.67
1.75-1.80
w-m

### Claim 23 (depends on 1)

A stable calcined form of the crystalline microporous metallophosphate of claim 1, AlPO-67C, comprising heating the metallophosphate of claim 1 under calcination conditions to remove the organic cations in the presence of air and ambient water vapor, said AlPO-67C comprising a three-dimensional framework of EO2−, PO2+ and at least one of [M2+O2]2− and SiO2 tetrahedral units characterized by the empirical formula:
HaMm2+EPxSiyOz
where M is at least one metal cation of valence +2 selected from the group consisting of Be2+, Mg2+, Zn2+, Co2+, Mn2+, Fe2+, Ni2+, “m” is the mole ratio of M to E and varies from 0 to about 1.0, H is a proton, “a” is the mole ratio of H to E and has a value of about 0.1 to about 2.0, E is an trivalent element selected from the group consisting of aluminum, gallium, iron, boron and mixtures thereof, “x” is mole ratio of P to E and varies from 0.5 to about 2.0, “y” is the mole ratio of Si to E and varies from 0 to about 1.0, “m”+“y”≧0.02, and “z” is the mole ratio of 0 to E and has a value determined by the equation:
z=(a+2·m+3+5·x+4·y)/2
and is characterized in that it has the x-ray diffraction pattern having at least the d-spacings and intensities set forth in Table B:
TABLE B
2Θ
d(Å)
I/I0%
9.02-8.33
9.80-10.6
w-m
11.09-10.79
7.97-8.19
vs
13.74-13.32
6.44-6.64
s-vs
17.58-16.97
5.04-5.22
m
21.19-20.69
4.19-4.29
m
22.32-21.87
3.98-4.06
m-s
28.78-28.13
3.10-3.17
m
32.78-32.05
2.73-2.79
w-m