# US 2013/0343971 A1 · Method for co-producing alumina and activated calcium silicate from high-alumina fly ash

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2013/0343971 A1
- Document ID: US20130343971A1
- Status: Published application
- Kind: A1
- Application number: 14/012,983
- Filed: 2013-08-28
- Published: 2013-12-26
- Earliest claimed: 2011-05-11
- Assignees: Inner Mongolia Datang International Recycling Resource Development Co., Ltd.
- Applicants: Inner Mongolia Datang International Recycling Resource Development Co., Ltd.
- Inventors: JUNMIN SUN; Zhanjun Zhang; Gang Chen; Shaoyong Yan; Qizhi Huo; Licheng Wu; Hongli Xu; Lian Qin; Xiaoxia Chen
- Web page: https://patentgrep.com/patent/US20130343971A1

## CPC

- C01B 33/24: Alkaline-earth metal silicates
- C01F 7/0693: from waste-like raw materials, e.g. fly ash or Bayer calcination dust
- C01F 7/085: according to the lime-sinter process
- C01F 7/30: Preparation of aluminium oxide or hydroxide by thermal decomposition or by hydrolysis or oxidation of aluminium compounds
- C01B: NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; {METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C}
- C01F: COMPOUNDS OF THE METALS BERYLLIUM, MAGNESIUM, ALUMINIUM, CALCIUM, STRONTIUM, BARIUM, RADIUM, THORIUM, OR OF THE RARE-EARTH METALS (metal hydrides {monoborane, diborane or addition complexes thereof} C01B6/00; salts of oxyacids of halogens C01B11/00; peroxides, salts of peroxyacids C01B15/00; sulfides or polysulfides of magnesium, calcium, strontium, or barium C01B17/42; thiosulfates, dithionites, polythionates C01B17/64; compounds containing selenium or tellurium C01B19/00; binary compounds of nitrogen with metals C01B21/06; azides C01B21/08; {compounds other than ammonia or cyanogen containing nitrogen and non-metals and optionally metals C01B21/082; amides or imides of silicon C01B21/087}; metal {imides or} amides C01B21/092, {C01B21/0923}; nitrites C01B21/50; {compounds of noble gases C01B23/0005}; phosphides C01B25/08; salts of oxyacids of phosphorus C01B25/16; carbides C01B32/90; compounds containing silicon C01B33/00; compounds containing boron C01B35/00; compounds having molecular sieve properties but not having base-exchange properties C01B37/00; compounds having molecular sieve and base-exchange properties, e.g. crystalline zeolites, C01B39/00; cyanides C01C3/08; salts of cyanic acid C01C3/14; salts of cyanamide C01C3/16; thiocyanates C01C3/20; {double sulfates of magnesium with sodium or potassium C01D5/12; with other alkali metals C01D15/00, C01D17/00})

## Abstract

A method for co-producing alumina and activated calcium silicate from high-alumina fly ash, comprising the steps that: high-alumina fly ash reacts with sodium hydroxide solution to obtain desiliconized solution and desiliconized fly ash; lime cream is added to the desiliconized solution to obtain activated calcium silicate; limestone and sodium carbonate solution are added to the desiliconized fly ash to blend raw slurry, the raw slurry is baked into clinker, and sodium aluminate crude solution is obtained from dissolution of the clinker; the sodium aluminate crude solution is subjected to the processes of first-stage deep desiliconization, second-stage deep desiliconization, carbonization decomposition, seed precipitation and etc to obtain alumina. According to the invention, less material flow and small amount of slag formation are achieved, the energy consumption, material consumption and production cost are low; the extraction rate of alumina is high, and meanwhile, activated calcium silicate with high added value is co-produced.

## Claims

### Claim 1

A method for co-producing alumina and activated calcium silicate from high-alumina fly ash, comprising the following steps:
1) pre-desiliconization: high-alumina fly ash and sodium hydroxide solution are mixed, then heated up and introduced into a pressure container for desiliconization reaction, and liquid phase desiliconized solution and solid phase fly ash filter cake are obtained by means of liquid-solid separation;
2) preparation of activated calcium silicate, which comprises the following steps:
a. lime cream is added to the desiliconized solution from step 1) for reaction, to obtain calcium silicate filter cake by means of filtering;
b. the calcium silicate filter cake is washed and then added with clean water to prepare a calcium silicate slurry, and lime cream is added to the calcium silicate slurry for dealkalization reaction; and
c. calcium silicate obtained from dealkalization reaction is washed with clean water and then added to dilute sulfuric acid for soaking; aluminum sulfate is added to decrease the pH to be below 10, soaking is then performed; and activated calcium silicate is obtained after washing, deslagging, filtering and drying;
3) preparation of raw slurry: sodium carbonate, limestone and/or quick lime solution are added to the fly ash filter cake to obtain a mixed slurry, and the mixed slurry is finely milled and blended into a raw slurry;
4) baking of clinker: the raw slurry is baked into clinker;
5) dissolution of clinker: the clinker and a first-stage regulating solution are mixed for first-stage dissolution to obtain a sodium aluminate crude solution and first-stage dissolution crude slag;
6) first-stage and second-stage deep desiliconization: sodium hydrate alumino-silicate seed crystal is added to the sodium aluminate crude solution for first-stage deep desiliconization to obtain a first-stage desiliconized refined solution, then a part of the first-stage desiliconized refined solution is subjected to second-stage deep desiliconization to obtain a second-stage desiliconized refined solution and second-stage deep desiliconization slag simultaneously;
7) carbonization decomposition, seed precipitation and baking of aluminum hydroxide: the second-stage desiliconized refined solution is subjected to carbonization decomposition to obtain aluminum hydroxide as seed crystal, the aluminum hydroxide is added to the first-stage desiliconized refined solution in step 6), which is not subjected to second-stage deep desiliconization, seed precipitation is carried out to obtain aluminum hydroxide, and alumina is obtained by baking the aluminum hydroxide.

### Claim 2 (depends on 1)

The method according to claim 1, characterized in that, the mass concentration of the sodium hydroxide solution in step 1) is 10-30%, the mass ratio of sodium hydroxide to high-alumina fly ash is 0.2-0.8:1, the reaction temperature is 70-135° C., and the reaction time is 0.5-3 hours.

### Claim 3 (depends on 1)

The method according to claim 1, characterized in that, the concentration of effective calcium oxide in the lime cream in step a is 100 g/L-220 g/L, the molar ratio of effective calcium oxide to SiO2 in filtrate is 0.7 to 1.2, the reaction temperature is 50-100° C., and the reaction time is 30-120 minutes.

### Claim 4 (depends on 1)

The method according to claim 1, characterized in that, the liquid-solid ratio of the calcium silicate slurry in step b is 2-6, the addition amount of the lime cream is that the mass ratio of effective calcium oxide in the lime cream to activated calcium silicate on dry basis is 20-80:1, and the dealkalization reaction time is 20-100 minutes.

### Claim 5 (depends on 1)

The method according to claim 1, characterized in that, the concentration of the dilute sulfuric acid in step c is 1/1000-10/1000, the mass ratio of activated calcium silicate on dry basis to concentrated sulfuric acid is 20-80:1, the soaking time is 10-60 minutes; the mass ratio of aluminum sulfate to activated calcium silicate on dry basis is 30-100:1, and the soaking time is 5-60 minutes.

### Claim 6 (depends on 1)

The method according to claim 1, characterized in that, the calcium ratio of the raw slurry in step 3) is 1.95-2.01, the sodium ratio is 0.95-1.05, and the water content is 25-50%.

### Claim 7 (depends on 1)

The method according to claim 1, characterized in that, the baking temperature in step 4) is 1150-1300° C., and the baking time is 10-60 minutes.

### Claim 8 (depends on 1)

The method according to claim 1, characterized in that, the grain diameter of the clinker during first-stage dissolution of step 5) is not more than 8 mm, the liquid-solid mass ratio of first-stage regulating solution to clinker is 2-8:1, the dissolution temperature is 55-85° C., the dissolution time is 5-30 minutes, the dissolution liquid is sodium aluminate crude solution, and the first-stage regulating solution contains the following ingredients: 10-60 g/L of Na2Ok, and 10-60 g/L of Na2Oc.

### Claim 9 (depends on 1)

The method according to claim 1, characterized in that, the conditions of first-stage deep desiliconization in step 6) are as follows: 10 g/L-100 g/L of sodium hydrate alumino-silicate, 100-180° C., and 0.5-5 hours; the conditions of second-stage deep desiliconization are as follows: 2 g/L-30 g/L of the addition amount of effective calcium oxide, 70-100° C., and 0.5-5 hours; and the volume ratio of the sodium aluminate crude solution, which is only subjected to first-stage deep desiliconization, to the sodium aluminate crude solution, which is subjected to both first-stage deep desiliconization and second-stage deep desiliconization, is 1-3:1.

### Claim 10 (depends on 1)

The method according to claim 1, characterized in that, the carbonization decomposition temperature of the second-stage desiliconized refined solution in step 7) is 85-90° C., and the carbonization decomposition rate is 85-93%.