# US 2013/0284692 A1 · Resin coated copper foil, method for manufacturing same and multi-layer circuit board

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2013/0284692 A1
- Document ID: US20130284692A1
- Status: Published application
- Kind: A1
- Application number: 13/757,857
- Filed: 2013-02-04
- Published: 2013-10-31
- Earliest claimed: 2012-04-28
- Assignees: Zhen Ding Technology Co., Ltd.
- Applicants: Zhen Ding Technology Co., Ltd.
- Inventors: MING-JAAN HO
- Web page: https://patentgrep.com/patent/US20130284692A1

## CPC

- H05K 1/0296: {Conductive pattern lay-out details not covered by sub groups H05K1/02 - H05K1/0295 (H05K1/11 takes precedence; lay-out adapted to mounted component configuration H05K1/18)}
- H05K 3/022: {Processes for manufacturing precursors of printed circuits, i.e. copper-clad substrates}
- H05K 3/386: {by the use of an organic polymeric bonding layer, e.g. adhesive}
- H05K 3/4626: {characterised by the insulating layers or materials (H05K3/4688 takes precedence)}
- H05K 3/4655: {by using a laminate characterized by the insulating layer (general-purpose insulating materials H05K1/03, H05K3/4673)}
- H05K 2201/0154: Polyimide
- H05K 2201/0358: Resin coated copper [RCC]
- Y10T 428/2804: Next to metal
- H05K: PRINTED CIRCUITS; CASINGS OR CONSTRUCTIONAL DETAILS OF ELECTRIC APPARATUS; MANUFACTURE OF ASSEMBLAGES OF ELECTRICAL COMPONENTS
- Y10T: TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION

## Abstract

A method for manufacturing a resin coating on copper foil includes following steps. Firstly, two diamines of 2,2-bis[4-(4-aminophenoxy)phenyl]propane and 4,4′-oxydianiline, and two acid anhydrides of pyromellitic diandydride and oxydiphthalic anhydride are added into a polar aprotic solvent and the solvent is stirred to form a mixed solution. Secondly, the mixed solution is heated to a temperature of about 170° C.-190° C. to allow a cross-linking reaction to be completed between the two diamines and the two acid anhydrides, thereby forming a thermoplastic polyimide adhesive fluid. The thermoplastic polyimide adhesive fluid is coated on a copper foil and cured to form a thermoplastic polyimide adhesive layer on the copper foil, thereby obtaining a resin coated copper foil. This disclosure also relates to resin coated copper foil and a method for manufacturing a multi-layer circuit board.

## Claims

### Claim 1

A method for manufacturing a resin coated copper foil, comprising:
adding diamines of 2,2-bis[4-(4-aminophenoxy)phenyl]propane and 4,4′-oxydianiline into a polar aprotic solvent, and adding acid anhydrides of pyromellitic diandydride and oxydiphthalic anhydride into the polar aprotic solvent to form a mixture, and stirring the mixture to form a second mixed solution;
heating the second mixed solution to a temperature of 170° C. to 190° C. to cause a cross-linking reaction between the diamines and the acid anhydrides, thereby forming a thermoplastic polyimide adhesive fluid; and
applying the thermoplastic polyimide adhesive fluid over a copper foil, and pre-curing the thermoplastic polyimide adhesive fluid to form a thermoplastic polyimide adhesive layer over the copper foil, thereby obtaining a resin coated copper foil.

### Claim 2 (depends on 1)

The method of claim 1, wherein the step of adding the diamines of 2,2-bis[4-(4-aminophenoxy)phenyl]propane and 4,4′-oxydianiline into a polar aprotic solvent, and adding acid anhydrides of pyromellitic diandydride and oxydiphthalic anhydride into the polar aprotic solvent to form a mixture comprises:
adding the diamines of 2,2-bis[4-(4-aminophenoxy)phenyl]propane and 4,4′-oxydianiline into the polar aprotic solvent to form a first mixture, and stirring the first mixture for a time period of from 40 minutes to 80 minutes at a room temperature to form a first mixed solution; and
adding the acid anhydrides of pyromellitic diandydride and oxydiphthalic anhydride into the first mixed solution to form a second mixture, and stirring the second mixture for a time period of 5 hours and 40 minutes to 6 hours and 20 minutes at a room temperature to form the second mixed solution.

### Claim 3 (depends on 1)

The method of claim 1, wherein an amount by weight of the pyromellitic diandydride in the second mixed solution is in the range from 1.3% to 1.5%, and an amount by weight of the oxydiphthalic anhydride in the second mixed solution is in the range from 5.9% to 6.1%.

### Claim 4 (depends on 3)

The method of claim 3, wherein an amount by weight of the 2,2-bis[4-(4-aminophenoxy)phenyl]propane in the second mixed solution is in the range from 1.2% to 1.3%, and an amount of the 4,4′-oxydianiline in the second mixed solution is in the range from 7.8% to 8.0%.

### Claim 5 (depends on 4)

The method of claim 4, wherein the polar aprotic solvent is N,N-dimethylacetamide, and an amount by weight of the N,N-dimethylacetamide in the second mixed solution is in the range from 83.1% to 83.8%.

### Claim 6 (depends on 1)

The method of claim 1, further comprising adding xylene to the second mixed solution, an amount by weight of the xylene in the second mixed solution is in the range from 3% to 8%, the xylene being added to the second mixed solution after forming the second mixed solution and before heating the second mixed solution.

### Claim 7 (depends on 1)

The method of claim 1, wherein the thermoplastic polyimide adhesive fluid is heated at a temperature of 110° C. to 130° C. for 20 minutes to 60 minutes.

### Claim 8 (depends on 1)

The method of claim 1, wherein the thermoplastic polyimide adhesive fluid is deaerated for about 24 hours or less than 24 hours in a vacuum machine to expel bubbles out of the polyimide adhesive fluid prior to applying the thermoplastic polyimide adhesive fluid over the copper foil.

### Claim 9 (depends on 1)

A resin coated copper foil, comprising a copper foil and a thermoplastic polyimide layer formed on the copper foil, the resin coated copper foil being formed using the method of claim 1.

### Claim 10 (depends on 9)

A method for manufacturing a multi-layer circuit board, comprising:
providing a core substrate, the core substrate comprising a first patterned electrically conductive layer, an insulation layer and a second patterned electrically conductive layer, the first and second patterned electrically conductive layers being arranged on opposite surfaces of the insulation layer;
stacking two resin coated copper foils of claim 9 respectively on the first and second patterned electrically conductive layers to form a preformed multi-layer board, the thermoplastic polyimide layers of the resin coated copper foils being respectively arranged adjacent to the first and second patterned electrically conductive layers;
heating and compressing the preformed multi-layer board to cure the thermoplastic polyimide layers; and
etching the copper foils of the resin coated copper foils to convert the copper foils into a third patterned electrically conductive layer and a fourth patterned electrically conductive layer, thereby obtaining a multi-layer circuit board.

### Claim 11 (depends on 10)

The method of claim 10, wherein a temperature for heating the multi-layer board is in the range from 220° C. to 240° C.

### Claim 12 (depends on 11)

The method of claim 11, wherein a pressure of pressing the multi-layer board is about 3 MPa, and a time period of heating and pressing the multi-layer board is in the range from 2 hours to 2.5 hours.