# US 2013/0284319 A1 · High Strength, High Toughness Steel Alloy

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2013/0284319 A1
- Document ID: US20130284319A1
- Status: Published application
- Kind: A1
- Application number: 13/457,631
- Filed: 2012-04-27
- Published: 2013-10-31
- Earliest claimed: 2012-04-27
- Inventors: Paul M. Novotny
- Web page: https://patentgrep.com/patent/US20130284319A1

## CPC

- C22C 38/46: with vanadium
- C21D 1/18: Hardening (C21D1/02 takes precedence); Quenching with or without subsequent tempering (quenching devices C21D1/62)
- C21D 6/001: {containing Ni (C21D6/004 takes precedence)}
- C21D 6/004: {containing Cr and Ni}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/005: {containing rare earths, i.e. Sc, Y, Lanthanides}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/34: with more than 1.5% by weight of silicon
- C22C 38/42: with copper
- C22C 38/44: with molybdenum or tungsten
- C22C 38/48: with niobium or tantalum
- C22C 38/58: with more than 1.5% by weight of manganese
- C21D 2211/008: Martensite
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)

## Abstract

A high strength, high toughness steel alloy is disclosed. The alloy has the following weight percent composition. Element C 0.30-0.55 Mn 0.6-1.75 Si 0.9-2.8 Cr 0.6-2.5 Ni 2.70-7.0 Mo + ½ W 0.25-1.3 Cu 0.30-1.25 Co 0.01 max. V + (5/9) × Nb 0.10-1.0 Ti 0.01 max. Al 0.015 max. Ca 0.005 max. The alloy further includes a grain refining element selected from the group consisting of 0.0001-0.01% Mg, 0.001-0.025% Y, and a combination thereof. The balance of the alloy is iron and usual impurities. Also disclosed is a hardened and tempered steel article having very high strength and fracture toughness and formed from the alloy set forth above. The alloy article according to this aspect of the invention is further characterized by being tempered at a temperature of about 500° F. to 600° F.

## Claims

### Claim 1

A high strength, high toughness steel alloy having good temper resistance, said alloy comprising, in weight percent, about:
C
0.30-0.55
Mn
0.6-1.75
Si
0.9-2.8
Cr
0.6-2.5
Ni
2.70-7.0
Mo + ½ W
0.25-1.3
Cu
0.3-1.25
Co
0.01 max.
V + (5/9) × Nb
0.1-1.0
Ti
0.01 max.
Al
0.015 max.
Ca
0.005 max.
a grain-refining element selected from the group consisting of 0.0001-0.01% Mg, 0.001-0.025% Y, and a combination thereof; and
the balance being iron and usual impurities wherein phosphorus is restricted to about 0.01% max. and sulfur is restricted to not more than about 0.001% max., and wherein
2≦(% Si+% Cu)/(% V+( 5/9)×% Nb)≦34.

### Claim 2 (depends on 1)

The alloy as set forth in claim 1 wherein the alloy contains at least about 0.002% yttrium.

### Claim 3 (depends on 2)

The alloy as set forth in claim 2 wherein the alloy contains not more than about 0.020% yttrium.

### Claim 4 (depends on 1)

The alloy as set forth in claim 1 wherein the alloy contains not more than about 0.006% magnesium.

### Claim 5 (depends on 1)

The alloy as set forth in claim 1 wherein the alloy contains not more than about 0.002% calcium.

### Claim 6 (depends on 1)

The alloy as set forth in claim 1 wherein the alloy contains at least about 0.35% carbon.

### Claim 7 (depends on 1)

The alloy as set forth in claim 1 wherein the alloy contains at least about 0.7% manganese.

### Claim 8 (depends on 7)

The alloy as set forth in claim 7 wherein the alloy contains not more than about 1.5% manganese.

### Claim 9 (depends on 1)

The alloy as set forth in claim 1 wherein the alloy contains at least about 1.2% silicon.

### Claim 10 (depends on 9)

The alloy as set forth in claim 9 wherein the alloy contains not more than about 2.7% silicon.

### Claim 11 (depends on 1)

The alloy as set forth in claim 1 wherein the alloy contains at least about 0.7% chromium.

### Claim 12 (depends on 11)

The alloy as set forth in claim 11 wherein the alloy contains not more than about 2.0% chromium.

### Claim 13 (depends on 1)

The alloy as set forth in claim 1 wherein the alloy contains not more than about 5.0% nickel.

### Claim 14 (depends on 1)

The alloy as set forth in claim 1 wherein Mo+½ W is at least about 0.4%.

### Claim 15 (depends on 14)

The alloy as set forth in claim 14 wherein Mo+½ W is not more than about 1.1%.

### Claim 16 (depends on 1)

The alloy as set forth in claim 1 wherein V+( 5/9)×Nb is at least about 0.25%.

### Claim 17 (depends on 1)

The alloy as set forth in claim 1 wherein
14.5≦(% Si+% Cu)/(% V+( 5/9) ×% Nb)≦34.

### Claim 18

A high strength, high toughness steel alloy having good temper resistance, said alloy comprising, in weight percent, about:
C
0.35-0.50
Mn
0.7-1.5
Si
1.2-2.7
Cr
0.7-2.0
Ni
2.75-5.0
Mo + ½ W
0.4-1.1
Cu
0.35-1.2
Co
0.01 max.
V + (5/9) × Nb
0.25-1.0
Ti
0.01 max.
Al
0.01 max.
Ca
0.002 max.
a grain-refining element selected from the group consisting of 0.0001-0.006% Mg, 0.002-0.020% Y, and a combination thereof; and
the balance being iron and usual impurities wherein phosphorus is restricted to about 0.01% max. and sulfur is restricted to not more than about 0.001% max., and wherein
14.5≦(% Si+% Cu)/(% V+( 5/9)×% Nb)≦34.

### Claim 19

A high strength, high toughness steel alloy having good temper resistance, said alloy comprising, in weight percent, about:
C
0.33-0.50
Mn
0.8-1.3
Si
1.0-2.70
Cr
1.5-1.8
Ni
3.0-5.0
Mo + ½ W
0.25-0.90
Cu
0.3-1.25
Co
0.01 max.
V + (5/9) × Nb
0.1-0.40
Ti
0.01 max.
Al
0.015 max.
Ca
0.001 max.
a grain-refining element selected from the group consisting of 0.0001-0.008% Mg, 0.002-0.025% Y, and a combination thereof; and
the balance being iron and usual impurities wherein phosphorus is restricted to about 0.01% max. and sulfur is restricted to not more than about 0.001% max., and wherein
14.5≦(% Si+% Cu)/(% V+( 5/9)×% Nb)≦34.

### Claim 20 (depends on 19)

The alloy as set forth in claim 19 wherein the alloy contains not more than about 0.45% carbon.

### Claim 21 (depends on 19)

The alloy as set forth in claim 19 wherein the alloy contains at least about 0.40% carbon.

### Claim 22 (depends on 19)

The alloy as set forth in claim 19 wherein the alloy contains not more than about 4.5% nickel.

### Claim 23 (depends on 19)

The alloy as set forth in claim 19 wherein the alloy contains at least about 4.0% nickel.

### Claim 24 (depends on 19)

The alloy as set forth in claim 19 wherein the alloy contains not more than about 1.2% copper.

### Claim 25 (depends on 19)

The alloy as set forth in claim 19 wherein the alloy contains not more than about 0.006% magnesium.

### Claim 26 (depends on 19)

The alloy as set forth in claim 19 wherein the alloy contains not more than about 0.020% yttrium.

### Claim 27

A high strength, high toughness steel alloy having good temper resistance, said alloy comprising, in weight percent, about:
C
0.33-0.45
Mn
0.8-1.3
Si
1.0-2.70
Cr
1.5-1.8
Ni
3.0-4.5
Mo + ½ W
0.25-0.90
Cu
0.35-1.25
Co
0.01 max.
V + (5/9) × Nb
0.10-0.40
Ti
0.01 max.
Al
0.015 max.
Ca
0.001 max.
a grain-refining element selected from the group consisting of 0.0001-0.006% Mg, 0.002-0.025% Y, and a combination thereof; and
the balance being iron and usual impurities wherein phosphorus is restricted to about 0.01% max. and sulfur is restricted to not more than about 0.001% max., and wherein
14.5≦(% Si+% Cu)/(% V+( 5/9)×% Nb)≦34.

### Claim 28

A high strength, high toughness steel alloy having good temper resistance, said alloy comprising, in weight percent, about:
C
0.40-0.50
Mn
0.8-1.3
Si
1.5-2.70
Cr
1.5-1.8
Ni
4.0-5.0
Mo + ½ W
0.25-0.90
Cu
0.3-1.2
Co
0.01 max.
V + (5/9) × Nb
0.10-0.40
Ti
0.01 max.
Al
0.015 max.
Ca
0.001 max.
a grain-refining element selected from the group consisting of 0.0001-0.008% Mg, 0.002-0.020% Y, and a combination thereof; and
the balance being iron and usual impurities wherein phosphorus is restricted to about 0.01% max. and sulfur is restricted to not more than about 0.001% max., and wherein
14.5≦(% Si+% Cu)/(% V+( 5/9)×% Nb)≦34.

### Claim 29 (depends on 1, 18, 19, 27)

A hardened and tempered article made from a high strength, high toughness steel alloy as set forth in any of claims 1, 18, 19, 27, and 28 wherein the article is tempered at a temperature of about 500° F. to 600° F.

### Claim 30 (depends on 29)

The hardened and tempered article as set forth in claim 29 which provides a room temperature tensile strength of at least about 295 ksi and a Charpy V-notch impact toughness of at least about 15 ft-lbs.