# US 2013/0279971 A1 · Electron-beam welded joint, steel for electron-beam welding, and manufacturing method

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2013/0279971 A1
- Document ID: US20130279971A1
- Status: Published application
- Kind: A1
- Application number: 13/988,737
- Filed: 2011-10-27
- Published: 2013-10-24
- Earliest claimed: 2010-11-22
- Assignees: Nippon Steel & Sumitomo Metal Corporation
- Inventors: Ryuichi Honma; Ryuji Uemori; Tadashi Ishikawa; Akihiko Kojima; Manabu Hoshino
- Web page: https://patentgrep.com/patent/US20130279971A1

## CPC

- B23K 35/3073: {with Mn as next major constituent}
- B23K 15/0093: {characterised by the properties of the materials to be welded}
- Y10T 403/477: Fusion bond, e.g., weld, etc.
- Y10T 428/12965: Both containing 0.01-1.7% carbon [i.e., steel]
- B23K: SOLDERING OR UNSOLDERING; WELDING; CLADDING OR PLATING BY SOLDERING OR WELDING; CUTTING BY APPLYING HEAT LOCALLY, e.g. FLAME CUTTING; WORKING BY LASER BEAM
- Y10T: TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION

## Abstract

An electron-beam welded joint including, by mass %, C: 0.02% to 0.1%, Si: 0.03% to 0.30%, Mn: 1.5% to 2.5%, Ti: 0.005 to 0.015%, N: 0.0020 to 0.0060%, O: 0.0010% to 0.0035%, Nb: 0% to 0.020%, V: 0% to 0.030%, Cr: 0% to 0.50%, Mo: 0% to 0.50%, Cu: 0% to 0.25%, Ni: 0% to 0.50%, B: 0% to 0.0030%, S: limited to 0.010% or less, P: limited to 0.015% or less, Al: limited to 0.004% or less, and a balance consisting of iron and unavoidable impurities, wherein an index value CeEB is 0.49% to 0.60%, a number of oxides having an equivalent circle diameter of 1.0 μm or more is 20 pieces/mm2 or less, and a number of oxides having an equivalent circle diameter of 0.05 μm or more and less than 0.5 μm is 1×103 pieces/mm2 to 1×105 pieces/mm2 at a thickness center portion.

## Claims

### Claim at position 1

1-8. (canceled)

### Claim 9

An electron-beam welded joint obtained by applying an electron-beam welding to a steel, the steel comprising as a composition, by mass %,
C: 0.02% to 0.10%,
Si: 0.03% to 0.30%,
Mn: 1.5% to 2.5%,
Ti: 0.005% to 0.015%,
N: 0.0020% to 0.0060%,
O: 0.0010% to 0.0035%
Nb: 0% to 0.020%,
V: 0% to 0.030%,
Cr: 0% to 0.50%,
Mo: 0% to 0.50%,
Cu: 0% to 0.25%,
Ni: 0% to 0.50%,
B: 0% to 0.0030%,
S: limited to 0.010% or less,
P: limited to 0.015% or less,
Al: limited to 0.004% or less, and
a balance consisting of iron and unavoidable impurities, wherein
an index value CeEB defined by a following Formula 1 is 0.49% to 060%,
a C/CeEB, which is a ratio of an amount in mass % of C in the steel relative to the index value CeEB of the steel, is 0.04 to 0.18,
a number of oxides having an equivalent circle diameter of 1.0 μm or more is 20 pieces/mm2 or less at a thickness center portion in a cross-section along a thickness direction of the steel, and
a number of oxides containing Ti of 10% or more and having an equivalent circle diameter of 0.05 μm or more and less than 0.5 μm is 1×103 pieces/mm2 to 1×105 pieces/mm2 at the thickness center portion,
the index value of hardenability after the electron-beam welding,
CeEB=C+(9/40)Mn+(1/15)Cu+(1/15)Ni+(1/5)Cr+(1/5)Mo+(1/5)V (Formula 1)
where C, Mn, Cu, Ni, Cr, Mo and V represent amounts in mass % of each element contained in the composition of the steel.

### Claim 10 (depends on 9)

The electron-beam welded joint according to claim 9, wherein the steel has a thickness of 45 to 150 mm.

### Claim 11 (depends on 9)

The electron-beam welded joint according to claim 9, wherein, when a CTOD value of a welded metal is defined as δWM, a CTOD value of a weld heat-affected zone is defined as δHAZ, and a CTOD value of the steel is defined as δBM,
0.5≦δWM/δBM≦1.1, and 0.5≦δHAZ/δBM≦1.1 are satisfied.

### Claim 12

A steel for an electron-beam welding, the steel comprising as a composition, by mass %,
C: 0.02% to 0.10%,
Si: 0.03% to 0.30%,
Mn: 1.5% to 2.5%,
Ti: 0.005% to 0.015%,
N: 0.0020% to 0.0060%,
O: 0.0010% to 0.0035%,
Nb: 0% to 0.020%,
V: 0% to 0.030%,
Cr: 0% to 0.50%,
Mo: 0% to 0.50%,
Cu: 0% to 0.25%,
Ni: 0% to 0.50%,
B: 0% to 0.0030%,
S: limited to 0.010% or less,
P: limited to 0.015% or less,
Al: limited to 0.004% or less, and
a balance consisting of iron and unavoidable impurities, wherein
an index value CeEB obtained by substituting the composition of the steel into a following Formula 1 is 0.49% to 0.60%,
a C/CeEB, which is a ratio of an amount in mass % of C in the steel relative to the index value CeEB of the steel, is 0.04 to 0.18,
a number of oxides having an equivalent circle diameter of 1.0 μm or more is 20 pieces/mm2 or less at a thickness center portion in a cross-section along a thickness direction of the steel, and
a number of oxides containing Ti of 10% or more and having an equivalent circle diameter of 0.05 μm or more and less than 0.5 μm is 1×103 pieces/mm2 to 1×105 pieces/mm2 at the thickness center portion,
the index value of hardenability after electron-beam welding,
CeEB=C+(9/40)Mn+(1/15)Cu+(1/15)Ni+(1/5)Cr+(1/5)Mo+(1/5)V (Formula 1)
where C, Mn, Cu, Ni, Cr, Mo, and V represent amounts in mass % of each element contained in the composition of the steel.

### Claim 13 (depends on 12)

The steel for the electron-beam welding according to claim 12, wherein the steel has a thickness of 45 to 150 mm.

### Claim 14 (depends on 12)

A method of manufacturing the steel for the electron-beam welding according to claim 12, the method comprising,
a casting process of casting and cooling the steel so that a cooling rate in a temperature range of 1300° C. to 1100° C. is 9° C./min or more, and
a process of heating the steel to a temperature range of 950° C. to 1150° C. after the casting process, and thereafter thermomechanical-treating the steel.

### Claim 15 (depends on 13)

A method of manufacturing the steel for the electron-beam welding according to claim 13, the method comprising,
a casting process of casting and cooling the steel so that a cooling rate in a temperature range of 1300° C. to 1100° C. is 9° C./min or more, and
a process of heating the steel to a temperature range of 950° C. to 1150° C. after the casting process, and thereafter thermomechanical-treating the steel.