# US 2013/0256598 A1 · Bismuth borate glass encapsulant for led phosphors

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2013/0256598 A1
- Document ID: US20130256598A1
- Status: Published application
- Kind: A1
- Application number: 13/852,048
- Filed: 2013-03-28
- Published: 2013-10-03
- Earliest claimed: 2012-03-30
- Assignees: Corning Incorporated
- Inventors: Bruce Gardiner Aitken; Michael Edward Badding; Nicholas Francis Borrelli; Nadja Teresia Lonnroth
- Web page: https://patentgrep.com/patent/US20130256598A1

## CPC

- C03C 14/006: {the non-glass component being in the form of microcrystallites, e.g. of optically or electrically active material}
- C03B 19/02: by casting {molten glass, e.g. injection moulding}
- C03B 19/06: by sintering, {e.g. by cold isostatic pressing of powders and subsequent sintering, by hot pressing of powders, by sintering slurries or dispersions not undergoing a liquid phase reaction}
- C03C 3/066: containing zinc
- C03C 3/068: containing rare earths
- C03C 3/14: containing boron
- C03C 3/145: containing aluminium or beryllium
- C03C 3/15: containing rare earths
- C03C 3/19: containing boron
- C03C 3/23: containing halogen and at least one oxide, e.g. oxide of boron
- C03C 3/247: containing fluorine and phosphorus
- C03C 4/12: for luminescent glass; for fluorescent glass
- C03C 8/24: Fusion seal compositions being frit compositions having non-frit additions, i.e. for use as seals between dissimilar materials, e.g. glass and metal; Glass solders
- C03C 17/007: {containing a dispersed phase, e.g. particles, fibres or flakes, in a continuous phase}
- C09K 11/02: Use of particular materials as binders, particle coatings or suspension media therefor
- C09K 11/7774: {Aluminates}
- C03B 2201/62: containing boron
- C03C 2204/00: Glasses, glazes or enamels with special properties
- C03C 2214/04: Particles; Flakes
- C03C 2214/16: Microcrystallites, e.g. of optically or electrically active material
- C03C 2217/452: Glass
- C03C 2217/47: consisting of a specific material
- C03C 2217/48: having a specific function
- H10H 20/851: Wavelength conversion means
- H10H 20/8511: {characterised by their material, e.g. binder}
- H10W 74/00: Encapsulations, e.g. protective coatings
- C03C: CHEMICAL COMPOSITION OF GLASSES, GLAZES OR VITREOUS ENAMELS; SURFACE TREATMENT OF GLASS; SURFACE TREATMENT OF FIBRES OR FILAMENTS MADE FROM GLASS, MINERALS OR SLAGS; JOINING GLASS TO GLASS OR OTHER MATERIALS
- C03B: MANUFACTURE, SHAPING, OR SUPPLEMENTARY PROCESSES
- C09K: MATERIALS FOR MISCELLANEOUS APPLICATIONS, NOT PROVIDED FOR ELSEWHERE
- H10H: INORGANIC LIGHT-EMITTING SEMICONDUCTOR DEVICES HAVING POTENTIAL BARRIERS
- H10W: GENERIC PACKAGES, INTERCONNECTIONS, CONNECTORS OR OTHER CONSTRUCTIONAL DETAILS OF DEVICES COVERED BY CLASS H10

## Abstract

Embodiments are directed to glass frits containing phosphors that can be used in LED lighting devices and for methods associated therewith for making the phosphor containing glass frit and their use in glass articles, for example, LED devices.

## Claims

### Claim 1

An article comprising a glass layer, wherein the layer comprises a glass comprising Bi2O3 and at least 30 mol % B2O3; and at least one phosphor, wherein the layer is a fired mixture of a frit comprising the Bi2O3 and B2O3 and the at least one phosphor.

### Claim 2 (depends on 1)

The article according to claim 1, wherein the layer is Pb free.

### Claim 3 (depends on 1)

The article according to claim 1, wherein the glass comprises in mole percent:
10-30% Bi2O3;
0-20% M2O, wherein M is Li, Na, K, Cs, or combinations thereof;
0-20% RO, wherein R is Mg, Ca, Sr, Ba, or combinations thereof;
15-50% ZnO, ZnF2, or a combination thereof;
0-5% Al2O3;
0-5% P2O5; and
30-55% B2O3.

### Claim 4 (depends on 3)

The article according to claim 3, comprising in mole percent:
10-30% Bi2O3;
greater than 0% Na2O;
15-50% ZnO, ZnF2, or a combination thereof;
30-55% B2O3;
0-3% SiO2;
0-1% WO3;
0-12% BaO, CaO, SrO, or combinations thereof.

### Claim 5 (depends on 4)

The article according to claim 4, comprising at least 1% Na2O.

### Claim 6 (depends on 4)

The article according to claim 4, comprising 15-50% ZnO.

### Claim 7 (depends on 4)

The article according to claim 4, comprising:
12-20% Bi2O3;
5-12% Na2O;
20-30% ZnO;
38-52% B2O3;
0-3% SiO2;
0-1% WO3;
1-12% BaO, CaO, SrO, or combinations thereof.

### Claim 8 (depends on 7)

The article according to claim 7, comprising:
14-16% Bi2O3;
5-11% Na2O;
22-27% ZnO;
40-51% B2O3;
0-3% SiO2;
0-1% WO3;
1-11% BaO, CaO, SrO, or combinations thereof.

### Claim 9 (depends on 8)

The article according to claim 8, wherein the glass has a refractive index of 1.81-1.83 at 473 nm and a glass transition temperature of 460° C. or less.

### Claim 10 (depends on 1)

The article according to claim 1, wherein the glass has a refractive index in the range of from 1.8 to 1.9.

### Claim 11 (depends on 1)

The article according to claim 1, wherein the glass has a glass transition temperature of 460° C. or less.

### Claim 12 (depends on 1)

The article according to claim 1, wherein the difference in refractive index between the frit and the at least one phosphor is ≦0.20.

### Claim 13 (depends on 1)

The article according to claim 1, further comprising a substrate having the glass layer disposed thereon.

### Claim 14 (depends on 13)

The article according to claim 13, wherein the CTE of the glass layer and the substrate are within ±2×10−6 of each other.

### Claim 15 (depends on 1)

The article according to claim 1, wherein the at least one phosphor has a quantum efficiency of greater than 90%.

### Claim 16 (depends on 1)

The article according to claim 1, wherein the glass layer has a total transmission of at least 60%.

### Claim 17 (depends on 1)

The article according to claim 1, wherein the glass layer thickness is about 100 microns.

### Claim 18 (depends on 1)

The article according to claim 1, wherein the at least one phosphor comprises less than 30% by weight of the glass layer.

### Claim 19

A method for making a glass article comprising:
providing a glass composition comprising Bi2O3 and at least 30 mol % B2O3;
melting the composition and forming the melted composition into a glass;
grinding the glass into particles to form a frit glass having the composition;
blending the frit glass with one or a more phosphors to form a phosphor-frit glass mixture;
converting the phosphor-frit glass mixture into a paste by adding at least one organic liquid to the mixture;
applying the paste onto a surface; and
firing the applied paste to burn out organic material to form a phosphor-frit glass.

### Claim 20 (depends on 19)

The method according to claim 19, further comprising cooling the fired phosphor-frit glass to room temperature after the firing.

### Claim 21 (depends on 19)

The method according to claim 19, wherein the firing comprises firing the applied paste in air to a temperature of approximately 350° C. at a temperature ramp rate of 2° C./min and holding the paste at approximately 350° C. for 1 hour to burn out the organic material.

### Claim 22 (depends on 19)

The method according to claim 19, wherein the firing comprises firing the applied paste in air to a selected temperature in the range of 475-600° C. at a temperature ramp rate of 2° C./min and holding the applied paste at the selected temperature for 2 hours.

### Claim 23 (depends on 19)

The method according to claim 19, wherein the applying comprises screen printing or tape casting the paste onto the surface.

### Claim 24 (depends on 19)

The method according to claim 19, wherein the blending comprises mixing the frit glass and the one or more phosphors with a solvent mixture comprising propylene glycol diacetate and dimethyl carbonate.

### Claim 25

A glass composition comprising in mole percent:
10-30% Bi2O3;
greater than 0% Na2O;
15-50% ZnO, ZnF2, or a combination thereof;
30-55% B2O3;
0-3% SiO2;
0-1% WO3;
0-12% BaO, CaO, SrO, or combinations thereof.

### Claim 26 (depends on 25)

The glass composition according to claim 25, comprising at least 1% Na2O.

### Claim 27 (depends on 25)

The glass composition according to claim 25, comprising 15-50% ZnO.

### Claim 28 (depends on 25)

The glass composition according to claim 25, comprising:
12-20% Bi2O3;
5-12% Na2O;
20-30% ZnO;
38-52% B2O3;
0-3% SiO2;
0-1% WO3;
1-12% BaO, CaO, SrO, or combinations thereof.

### Claim 29 (depends on 28)

The glass composition according to claim 28, comprising:
14-16% Bi2O3;
5-11% Na2O;
22-27% ZnO;
40-51% B2O3;
0-3% SiO2;
0-1% WO3;
1-11% BaO, CaO, SrO, or combinations thereof.

### Claim 30 (depends on 25)

The glass composition according to claim 25, having a refractive index of 1.81-1.83 at 473 nm and a glass transition temperature of 460° C. or less.

### Claim 31

A solid glass layer comprising a glass matrix and at least one phosphor dispersed throughout the matrix, wherein the glass comprises Bi2O3 and at least 30 mol % B2O3.

### Claim 32 (depends on 31)

The solid glass layer according to claim 31, wherein a minimum in a thickness-normalized absorbance of the glass layer occurs at a wavelength of less than 416 nm.

### Claim 33 (depends on 1)

The article according to claim 1, wherein the at least one phosphor is a quantum dot.