# US 2013/0253125 A1 · High flow and stiff polymer material with good transparency and impact properties

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2013/0253125 A1
- Document ID: US20130253125A1
- Status: Published application
- Kind: A1
- Application number: 13/823,249
- Filed: 2011-09-12
- Published: 2013-09-26
- Earliest claimed: 2010-09-16
- Assignees: Borealis AG
- Inventors: Cornelia Kock; Christelle Grein; Floran Prades
- Web page: https://patentgrep.com/patent/US20130253125A1

## CPC

- C08L 23/14: Copolymers of propene (C08L23/16 takes precedence)
- C08F 210/06: Propene
- C08L 23/10: Homopolymers or copolymers of propene
- C08L 23/12: Polypropene
- C08K 5/0083: {Nucleating agents promoting the crystallisation of the polymer matrix}
- C08L 23/06: Polyethylene
- C08L 23/0815: {with aliphatic 1-olefins containing one carbon-to-carbon double bond}
- C08L 23/16: Ethylene-propylene or ethylene-propylene-diene copolymers
- C08L 2205/025: containing two or more polymers of the same hierarchy C08L, and differing only in parameters such as density, comonomer content, molecular weight, structure
- C08L 2205/03: containing three or more polymers in a blend
- C08L 2205/035: containing four or more polymers in a blend
- C08L 2207/02: Heterophasic composition
- C08L 2308/00: Chemical blending or stepwise polymerisation process with the same catalyst
- C08L 2666/04: Macromolecular compounds according to groups C08L7/00 - C08L49/00, or C08L55/00 - C08L57/00; Derivatives thereof
- C08L: COMPOSITIONS OF MACROMOLECULAR COMPOUNDS (compositions based on polymerisable monomers C08F, C08G; artificial filaments or fibres D01F; textile treating compositions D06)
- C08F: MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
- C08K: Use of inorganic or non-macromolecular organic substances as compounding ingredients (paints, inks, varnishes, dyes, polishes, adhesives C09)

## Abstract

Polypropylene composition having a melt flow rate MFR2 (230° C.) of equal or above 15 g/10 min comprising: (a) a crystalline polypropylene matrix; (b) an elastomeric propylene copolymer phase having a propylene content in the range of 40 to 80 wt.-%, and an intrinsic viscosity in the range of more than 0.7 to less or equal 2.5 dl/g; (c) a first polyethylene having a density in the range 905 to 925 kg/m3 and melt flow rate MFR2 (190° C.) of below 30 g/10 min; (d) a second polyethylene having a density of above 915 kg/m3, and a melt flow rate MFR2 (190° C.) of equal or above 30 g/10 min.

## Claims

### Claim 1

Polypropylene composition having a melt flow rate MFR2 (230° C.) measured according to ISO 1133 of equal or above 15 g/10 min comprising
(a) a crystalline polypropylene matrix (M-PP)
(b) an elastomeric propylene copolymer phase (E) having
(i) a propylene content in the range of 40 to 80 wt.-%, and
(ii) an intrinsic viscosity (IV) measured according to ISO 1628-1 (at 135° C. in decalin) in the range of more than 0.7 to less or equal 2.5 dl/g,
(c) a first polyethylene (PE1) having
(i) a density measured according to ISO 1183-187 in the range 905 to 925 kg/m3, and
(ii) a melt flow rate MFR2 (190° C.) measured according to ISO 1133 of below 30 g/10 min,
(d) a second polyethylene (PE2) having
(i) a density measured according to ISO 1183-187 of above 915 kg/m3, and
(ii) a melt flow rate MFR2 (190° C.) measured according to ISO 1133 of equal or above 30 g/10 min.

### Claim 2 (depends on 1)

Polypropylene composition according to claim 1, wherein the crystalline polypropylene matrix (M-PP) has
(a) a melt flow rate MFR2 (230° C.) measured according to ISO 1133 in the range of 30 to 100 g/10 min,
and/or
(b) has a xylene cold soluble content (XCS) of equal or below 4.0 wt.-%,
and/or
(c) a melting temperature Tm determined by differential scanning calorimetry (DSC) of at least 145° C.

### Claim 3 (depends on 1)

Polypropylene composition according to claim 1, wherein the crystalline polypropylene matrix (M-PP)
(a) has a comonomer content of equal or below 4.0 wt.-%,
and/or
(b) comprises at least two different crystalline polypropylene fractions, said fractions differ in the comonomer content.

### Claim 4 (depends on 3)

Polypropylene composition according to claim 3, wherein the crystalline polypropylene matrix (M-PP) comprises
(a) at least one propylene homopolymer fraction and/or at least one random propylene copolymer fraction,
and/or
(b) one propylene homopolymer (H-PP) and one random propylene copolymer (R-PP), wherein further the weight ratio (H-PP/R-PP) between the propylene homopolymer (H-PP) and the random propylene copolymer n (R-PP) is preferably 70/30 to 30/70.

### Claim 5 (depends on 1)

Polypropylene composition according to claim 1, wherein the elastomeric propylene copolymer phase (E) comprises a first elastomeric propylene copolymer (E1) and a second elastomeric propylene copolymer (E2), the first elastomeric propylene copolymer (E1) and the second elastomeric propylene copolymer (E2) differ in their intrinsic viscosity measured according to ISO 1628-1 (at 135° C. in decalin).

### Claim 6 (depends on 5)

Polypropylene composition according to claim 5, wherein the weight ratio (E1/E2) between the first elastomeric propylene copolymer (E1) and the second elastomeric propylene copolymer (E2) is 80/20 to 20/80.

### Claim 7 (depends on 5)

Polypropylene composition according to claim 5, wherein the first elastomeric propylene copolymer (E1) has
(i) a propylene content in the range of 25 to 60 wt.-%, and
(ii) an intrinsic viscosity (IV) measured according to ISO 1628-1 (at 135° C. in decalin) in the range of equal to or more than 0.5 to 2.5 dl/g.

### Claim 8 (depends on 5)

Polypropylene composition according to claim 5, wherein the second elastomeric propylene copolymer (E2) has
(i) a propylene content in the range of 50 to 85 wt.-%, and
(ii) an intrinsic viscosity (IV) measured according to ISO 1628-1 (at 135° C. in decalin) in the range of equal to or more than 1.0 to below 3.0 dl/g.

### Claim 9 (depends on 1)

Polypropylene composition according to claim 1, wherein the first polyethylene (PE1) has
(a) an ethylene content of at least 80 wt.-%,
and/or
(b) a molecular weight distribution determined by gel permeation chromatography (GPC) of at least 10.

### Claim 10 (depends on 1)

Polypropylene composition according to claim 1, wherein the second polyethylene (PE2) has
(a) an ethylene content of at least 80 wt.-%,
and/or
(b) a molecular weight distribution determined by gel permeation chromatography (GPC) of below 10.

### Claim 11 (depends on 5)

Polypropylene composition according to claim 5, wherein the elastomeric propylene copolymer phase (E) is, preferably the first elastomeric propylene copolymer (E1) and the second elastomeric propylene copolymer (E2), dispersed within the crystalline polypropylene matrix (M-PP).

### Claim 12 (depends on 1)

Polypropylene composition according to claim 1, wherein the polypropylene composition comprises additionally an α-nucleating agent (NA).

### Claim 13 (depends on 1)

Polypropylene composition according to claim 1, wherein the composition comprises
(a1) 55 to 80 wt.-% of the crystalline polypropylene matrix (M-PP)
(b1) 7.5 to 30 wt.-% of the elastomeric propylene copolymer phase (E),
(e1) 2.5 to 15 wt.-% of the first polyethylene (PE1),
(d1) 2.5 to 15 wt.-% of the second polyethylene (PE2), and
(e1) 0.0005 to 1.0 wt.-% of a α-nucleating agent (NA),
or
(a2) 55 to 80 wt.-% of the crystalline polypropylene matrix (M-PP)
(b2) 2.5 to 20 wt.-% of a first elastomeric propylene copolymer (E1),
(c2) 2.5 to 20 wt.-% of a second elastomeric propylene copolymer (E2),
(d2) 2.5 to 15 wt.-% of the first polyethylene (PE1),
(e2) 2.5 to 15 wt.-% of the second polyethylene (PE2), and
(f2) 0.0005 to 1.0 wt.-% of a α-nucleating agent (NA),
or
(a3) 15 to 55 wt.-% of a first crystalline polypropylene fraction being part of the crystalline polypropylene matrix (M-PP),
(b3) 15 to 55 wt.-% of a second crystalline polypropylene fraction being part of the crystalline polypropylene matrix (M-PP)
(c3) 2.5 to 20 wt.-% of a first elastomeric propylene copolymer (E1),
(d3) 2.5 to 20 wt.-% of a second elastomeric propylene copolymer (E2),
(e3) 2.5 to 15 wt.-% of the first polyethylene (PE1),
(f3) 2.5 to 15 wt.-% of the second polyethylene (PE2), and
(g3) 0.0005 to 1.0 wt.-% of a α-nucleating agent (NA).

### Claim 14

Injection molded article comprising a polypropylene composition having a melt flow rate MFR2 (230° C.) measured according to ISO 1133 of equal or above 15 g/10 min comprising
(a) a crystalline polypropylene matrix (M-PP)
(b) an elastomeric propylene copolymer phase (E) having
(i) a propylene content in the range of 40 to 80 wt.-%, and
(ii) an intrinsic viscosity (IV) measured according to ISO 1628-1 (at 135° C. in decalin) in the range of more than 0.7 to less or equal 2.5 dl/g,
(c) a first polyethylene (PE1) having
(i) a density measured according to ISO 1183-187 in the range 905 to 925 kg/m3, and
(ii) a melt flow rate MFR2 (190° C.) measured according to ISO 1133 of below 30 g/10 min,
(d) a second polyethylene (PE2) having
(i) a density measured according to ISO 1183-187 of above 915 kg/m3, and
(ii) a melt flow rate MFR2 (190° C.) measured according to ISO 1133 of equal or above 30 g/10 min.

### Claim 15

Process for the preparation of polypropylene composition having a melt flow rate MFR2 (230° C.) measured according to ISO 1133 of equal or above 15 g/10 min comprising
(a) a crystalline polypropylene matrix (M-PP)
(b) an elastomeric propylene copolymer phase (E) having
(i) a propylene content in the range of 40 to 80 wt.-%, and
(ii) an intrinsic viscosity (IV) measured according to ISO 1628-1 (at 135° C. in decalin) in the range of more than 0.7 to less or equal 2.5 dl/g,
(c) a first polyethylene (PE1) having
(i) a density measured according to ISO 1183-187 in the range 905 to 925 kg/m3, and
(ii) a melt flow rate MFR2 (190° C.) measured according to ISO 1133 of below 30 g/10 min,
(d) a second polyethylene (PE2) having
(i) a density measured according to ISO 1183-187 of above 915 kq/m3, and
(ii) a melt flow rate MFR2 (190° C.) measured according to ISO 1133 of equal or above 30 g/10 min;
comprising the steps of mixing up a composition comprising the polypropylene matrix (M-PP) and the elastomeric propylene copolymer phase (E), the first polyethylene (PE1), of the second polyethylene (PE2), and optionally a α-nucleating agent (NA) in an extruder.