# US 2013/0251298 A1 · Rolling Element Bearing and Method of Making the Same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2013/0251298 A1
- Document ID: US20130251298A1
- Status: Published application
- Kind: A1
- Application number: 13/677,860
- Filed: 2012-11-15
- Published: 2013-09-26
- Earliest claimed: 2012-03-20
- Assignees: Aktiebolaget Skf
- Applicants: Aktiebolaget Skf
- Inventors: Juergen Gegner; Wolfgang Nierlich; Armin Olschewski; Kenred Stadler; Arno Stubenrauch; Markus Volkmuth
- Web page: https://patentgrep.com/patent/US20130251298A1

## CPC

- F16C 43/04: Assembling rolling-contact bearings
- C21D 9/40: for rings; for bearing races
- C22C 1/02: by melting {(C22C1/1036 takes precedence)}
- F16C 19/16: with a single row of balls
- F16C 33/60: divided {or split, e.g. comprising two juxtaposed rings}
- F16C 33/62: Selection of substances
- F16C 33/64: Special methods of manufacture
- F16C 2223/00: Surface treatments; Hardening; Coating
- F16C 2223/10: Hardening, e.g. carburizing, carbo-nitriding
- F16C 2223/18: with induction hardening
- F16C 2240/18: Stress
- Y10T 29/49636: Process for making bearing or component thereof
- Y10T 29/49689: Race making
- Y10T 29/49707: Bearing surface treatment
- Y10T 29/49709: Specific metallic composition
- F16C: SHAFTS; FLEXIBLE SHAFTS; ELEMENTS OR CRANKSHAFT MECHANISMS; ROTARY BODIES OTHER THAN GEARING ELEMENTS; BEARINGS
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- Y10T: TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION

## Abstract

A method for manufacturing a rolling-element bearing includes forming an inner ring from a steel having a sulfur content of 0.002 to 0.015 mass % and an oxygen content of less than 15 ppm, subjecting the inner ring to a hardening heat treatment that ends by performing a final heat treatment step at a predetermined temperature, cold working the inner-ring raceway to generate compressive residual stresses at least in a surface layer of the inner-ring raceway, subjecting the inner ring to a bluing treatment and subjecting the blued inner ring to a thermal post-treatment process at a temperature below the predetermined temperature of the final hardening heat treatment step. The resulting rolling-element bearing may exhibit compressive residual stresses having an absolute value of at least 200 MPa at 0.1 mm beneath the outer surface of the inner-ring raceway and a maximum value of 1500 MPa or less throughout the inner ring.

## Claims

### Claim 1

A method for manufacturing a rolling-element bearing, which includes an inner ring having an inner-ring raceway, an outer ring having an outer-ring raceway and a plurality of rolling elements that are rollable on the inner-ring raceway and on the outer-ring raceway, the method comprising:
forming the inner ring from a steel having a sulfur content of 0.002 to 0.015 mass % and an oxygen content of less than 15 ppm,
subjecting the inner ring to a heat treatment to harden it, which heat treatment ends by performing a final hardening heat treatment step at a predetermined temperature,
cold working the inner-ring raceway to generate compressive residual stresses at least in a surface layer of the inner-ring raceway,
subjecting the cold-worked inner ring to a bluing treatment to form a blued layer on an outer surface of the inner ring, and
subjecting the blued inner ring to a thermal post-treatment process at a temperature below the predetermined temperature of the final hardening heat treatment step.

### Claim 2 (depends on 1)

The method according to claim 1, wherein the hardening heat treatment step comprises subjecting the inner ring to martensitic, case and/or induction hardening and
wherein the predetermined temperature of the final hardening heat treatment step is a tempering temperature of the inner ring.

### Claim 3 (depends on 2)

The method according to claim 2, wherein a retained austenite content of 8 to 18 volume % is formed in the inner ring by the martensitic, case, and/or induction hardening.

### Claim 4 (depends on 1)

The method according to claim 1, wherein the hardening heat treatment step comprises subjecting the inner ring to bainitic hardening, and
wherein the predetermined temperature of the final heat treatment step is a bainitic transformation temperature of the inner ring.

### Claim 5 (depends on 1)

The method according to claim 1, wherein the cold working step is performed such that compressive residual stresses are formed in the inner ring up to a minimum depth beneath the outer surface of the inner-ring raceway with an absolute value of a minimum value or greater, the minimum depth being 0.1 mm and the minimum value being at least 200 MPa.

### Claim 6 (depends on 5)

The method according to claim 5, wherein the minimum depth is 0.2 mm and the minimum value is 400 MPa or more.

### Claim 7 (depends on 1)

The method according to claim 1, wherein the cold working step is performed such that compressive residual stresses formed in the inner ring have a maximum absolute value of 1500 MPa or less.

### Claim 8 (depends on 7)

The method according to claim 7, wherein the maximum absolute value is 800 MPa or less

### Claim 9 (depends on 1)

The method according to claim 1, wherein the temperature of the thermal post-treatment process is at least 10 K below the predetermined temperature of the final hardening heat treatment step.

### Claim 10 (depends on 9)

The method according to claim 9, wherein the temperature of the thermal post-treatment process is at least 100° C.

### Claim 11 (depends on 10)

The method according to claim 10, wherein the temperature of the thermal post-treatment process is no more than 100 K below the predetermined temperature of the final hardening heat treatment step.

### Claim 12 (depends on 1)

The method according to claim 1, wherein the temperature of the final hardening heat treatment step is higher than temperatures of the cold working, the bluing treatment and the thermal post-treatment process.

### Claim 13 (depends on 1)

The method according to claim 1, wherein the inner ring is formed from a steel having a sulfur content of 0.006 to 0.015 mass % and an oxygen content of less than 10 ppm.

### Claim 14 (depends on 1)

The method according to claim 1, wherein the inner ring is formed from a steel that comprises 0.65-1.20 wt % C, 0.05-1.70 wt % Si, 1.1-2.2 wt % Cr, 0.10-1.0 wt % Mn, 0.02-1.0 wt % Ni, 0.02-0.70 wt % Mo.

### Claim 15

A method for manufacturing a rolling-element bearing, which includes an inner ring having an inner-ring raceway, an outer ring having an outer-ring raceway and a plurality of rolling elements that are rollable on the inner-ring raceway and on the outer-ring raceway, the method comprising:
forming the inner ring from a steel having a sulfur content of 0.006 to 0.015 mass % and an oxygen content of less than 10 ppm, the inner ring having an inner diameter of at least 50 centimeters,
subjecting the inner ring to a hardening heat treatment that ends by performing a final hardening heat treatment step at a predetermined temperature,
cold working the inner-ring raceway to generate compressive residual stresses at least in a surface layer of the inner-ring raceway, the compressive residual stresses having an absolute value of at least 500 MPa at 0.2 mm beneath an outer surface of the inner-ring raceway and a maximum value of 800 MPa or less throughout the inner ring,
subjecting the cold-worked inner ring to a bluing treatment to form a blued layer on an outer surface of the inner-ring raceway, and
subjecting the blued inner ring to a thermal post-treatment process at a temperature of at least 100° C. and between 10-100° C. below the predetermined temperature of the final hardening heat treatment step.

### Claim 16 (depends on 15)

The method according to claim 15, wherein:
the inner ring is formed from a steel that comprises 0.8-1.20 wt % C, 0.05-1.70 wt % Si, 1.1-2.2 wt % Cr, 0.10-1.0 wt % Mn, 0.02-1.0 wt % Ni, 0.02-0.70 wt % Mo;
the hardening heat treatment is a bainite transformation performed at a temperature between 210-240° C.; and
the thermal post-treatment process is performed at a temperature between 190-230° C.

### Claim 17 (depends on 16)

A rolling-element bearing produced by the method of claim 16.

### Claim 18 (depends on 1)

A rolling-element bearing produced by the method of claim 1.

### Claim 19

A rolling-element bearing, comprising:
an inner ring having an inner-ring raceway, the inner ring being comprised of a steel having a sulfur content of 0.002 to 0.015 mass % and an oxygen content of less than 15 ppm,
an outer ring having an outer-ring raceway and
a plurality of rolling elements contacting the inner-ring raceway and the outer-ring raceway,
wherein the inner ring has been hardened by a heat treatment, has compressive residual stresses in a surface region thereof generated by cold working, and includes a blued layer formed on its outer surface that has been subjected to thermal post-treatment.

### Claim 20 (depends on 19)

The rolling-element bearing according to claim 19, wherein:
the inner ring is formed from a steel that comprises 0.8-1.20 wt % C, 0.05-1.70 wt % Si, 1.1-2.2 wt % Cr, 0.10-1.0 wt % Mn, 0.02-1.0 wt % Ni, 0.02-0.70 wt % Mo and has a sulfur content of 0.006 to 0.015 mass % and an oxygen content of less than 10 ppm; and
the compressive residual stresses exhibit an absolute value of at least 500 MPa at 0.2 mm beneath the outer surface of the inner-ring raceway and a maximum value of 800 MPa or less throughout the inner ring.