# US 2013/0158220 A1 · Method Of Manufacture Of Polytetrafluoroethylene Stretched Film, And Polytetrafluoroethylene Stretched Film

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2013/0158220 A1
- Document ID: US20130158220A1
- Status: Published application
- Kind: A1
- Application number: 13/818,651
- Filed: 2011-08-19
- Published: 2013-06-20
- Earliest claimed: 2010-08-26
- Assignees: National University Corporation Gunma University
- Inventors: Hiroki Uehara; Takeshi Yamanobe; Yasumasa Yukawa; Yasuhiko Matsuoka
- Web page: https://patentgrep.com/patent/US20130158220A1

## CPC

- B29C 43/14: in several steps
- B29C 43/003: {characterised by the choice of material}
- B29C 43/006: {Pressing and sintering powders, granules or fibres}
- B29C 48/0018: {combined with shaping by orienting, stretching or shrinking, e.g. film blowing (B29C48/0017 takes precedence)}
- B29C 48/92: Measuring, controlling or regulating
- B29C 55/00: Shaping by stretching, e.g. drawing through a die; Apparatus therefor (B29C61/08 takes precedence)
- B29C 55/12: biaxial
- B29C 55/16: simultaneously
- C08J 5/18: Manufacture of films or sheets
- C08L 27/18: Homopolymers or copolymers or tetrafluoroethene
- B29C 48/022: {characterised by the choice of material}
- B29C 48/10: flexible, e.g. blown foils
- B29C 2043/3605: {vacuum}
- B29C 2043/366: {plates pressurized by an actuator, e.g. ram drive, screw, vulcanizing presses}
- B29C 2043/561: {under vacuum conditions}
- B29C 2948/92266: Mechanical properties
- B29C 2948/92514: Pressure
- B29C 2948/92704: Temperature
- B29C 2948/92761: Mechanical properties
- B29K 2027/18: PTFE, i.e. polytetrafluoroethylene {, e.g. ePTFE, i.e. expanded polytetrafluoroethylene}
- B29K 2995/0053: bi-axially
- C08J 2327/18: Homopolymers or copolymers of tetrafluoroethylene
- C08L 2205/02: containing two or more polymers of the same C08L -group
- B29C: SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING (making preforms B29B11/00; making laminated products by combining previously unconnected layers which become one product whose layers will remain together B32B37/00 - B32B41/00)
- C08J: WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H (working, e.g. shaping, of plastics B29)
- C08L: COMPOSITIONS OF MACROMOLECULAR COMPOUNDS (compositions based on polymerisable monomers C08F, C08G; artificial filaments or fibres D01F; textile treating compositions D06)
- B29K: INDEXING SCHEME ASSOCIATED WITH SUBCLASSES B29B, B29C OR B29D, RELATING TO MOULDING MATERIALS OR TO MATERIALS FOR {MOULDS, } REINFORCEMENTS, FILLERS OR PREFORMED PARTS, e.g. INSERTS

## Abstract

A method of manufacturing a PTFE stretched film that has higher tensile strength at its breaking point. In the method, a resin composition is obtained by mixing an emulsion of PTFE (A) with a number average molecular weight of 5×106 or more and an emulsion of PTFE (B) with a number average molecular weight of 1×106 to 4×106 so that the solid content ratio (A/B) of the PTFE (A) and the PTFE (B) is 99/1 to 10/90. The mixed emulsion is subjected to compression molding in a melted state under a reduced-pressure atmosphere to obtain a film.

## Claims

### Claim 1

A method of manufacture of polytetrafluoroethylene stretched film having the following steps (I) and (II),
(I) A step in which a resin composition obtained by mixing an emulsion of polytetrafluoroethylene (A) with a number average molecular weight of 5×106 or more and an emulsion of polytetrafluoroethylene (B) with a number average molecular weight of 1×106 to 4×106 so that the solid content ratio (A/B) of the polytetrafluoroethylene (A) and the polytetrafluoroethylene (B) is 99/1 to 10/90 is subjected to compression molding in a melted state under a reduced-pressure atmosphere to obtain a film and
(II) A step in which said film is melt stretched,
wherein said melt stretching is biaxial stretching,
said step (I) has a step (I-1) in which said resin composition is pressed at the first pressure V1 (0.01-100 MPa) for 1-100 minutes in a state where it has been heated to a temperature T1 (15-150° C.) under a reduced-pressure atmosphere, and a step (I-2) in which the heated and pressed resin composition in said step (I-1) is further heated at a temperature T2 (330-420° C.) to a melted state, and compression molded at a the second pressure V2 (0.01-100 MPa) for 1-100 minutes under a reduced-pressure atmosphere,
said reduced-pressure atmosphere in said steps (I) and (II) is 10 Torr or less, and
the difference of said second pressure V2 and said first pressure V1 (V2−V1) ranges between about 0.1-99 MPa.

### Claim 2

(canceled)

### Claim 3 (depends on 1)

A method of manufacture of polytetrafluoroethylene stretched film according to claim 1, wherein said step (I) additionally has a step (I-3) in which molded film is obtained by allowing cooling to being kept in a pressed state under a reduced-pressure atmosphere (10 Torr or less).

### Claim 4 (depends on 1)

The method of manufacture of polytetrafluoroethylene stretched film according to claim 1, wherein an average particle size of the polytetrafluoroethylene (A) in the emulsion of polytetrafluoroethylene (A) is within the range of about 0.03-0.5 μm, and an average particle size of the polytetrafluoroethylene (B) in the emulsion of polytetrafluoroethylene (B) is within the range of about 0.03-0.5 μm.

### Claim at position 5

5-7. (canceled)

### Claim 8 (depends on 1)

The method of manufacture of polytetrafluoroethylene stretched film according to claim 1, wherein the pre-melted resin composition used in said step (I) is in powder form.

### Claim 9 (depends on 1)

The method of manufacture of polytetrafluoroethylene stretched film according to claim 1, wherein said polytetrafluoroethylene (A) and polytetrafluoroethylene (B) are polytetrafluoroethylene obtained by emulsion polymerization.

### Claim 10 (depends on 9)

The method of manufacture of PTFE stretched film according to claim 9, wherein a polymerization temperature is about 10-95° C., a polymerization pressure is about 0.5-4.0 MPa, and a polymerization time is about 90-520 minutes in said emulsion polymerization.

### Claim 11 (depends on 1)

The method of manufacture of polytetrafluoroethylene stretched film according to claim 1, wherein a temperature at which the film is in a melted state in said step (II) is within the range of about 330-420° C.

### Claim 12

(canceled)

### Claim 13 (depends on 1)

The method of manufacture of polytetrafluoroethylene stretched film according to claim 1, wherein said biaxial stretching is simultaneous biaxial stretching in which said film is in a melted state by hot-air blowing, and two axes are simultaneously stretched.

### Claim 14 (depends on 13)

The method of manufacture of polytetrafluoroethylene stretched film according to claim 13, wherein a stretching ratio is about 2.5-fold or more in said simultaneous biaxial stretching.

### Claim 15

(canceled)

### Claim 16 (depends on 1)

The method of manufacture of polytetrafluoroethylene stretched film according to claim 1, wherein said melt stretching is biaxial stretching and conducted in conditions as follows:
temperature: 330-420° C.
stretching speed: 1-1000 mm/minute, and
stretching ratio (vertical and horizontal directions): 1.1-10 fold and 1.1-10 fold.

### Claim 17 (depends on 16)

The method of manufacture of polytetrafluoroethylene stretched film according to claim 16, wherein said melt stretching is conducted in conditions as follows:
temperature: 380° C.,
stretching speed: 30 mm/minute,
stretching ratio (vertical and horizontal directions): 2.4-2.9 fold and 2.4-2.9 fold, said step (I-1) is conducted in conditions as follows:
reduced pressure atmosphere: 1×10−1 Torr or less,
pressing: 2.2MPa (the first pressure V1) for 10 minutes,
said step (I-2) is conducted in conditions as follows:
reduced pressure atmosphere: 1×10−1 Torr or less,
pressing: 2.9 MPa (the first pressure V2) for 5 minutes, and
the difference of said second pressure V2 and said first pressure V1 (V2−V1) is 0.7 MPa.

### Claim 18

Polytetrafluoroethylene stretched film, which is manufactured by the polytetrafluoroethylene stretched film manufacturing method having the following steps (I) and (II),
(I) a step in which a resin composition obtained by mixing an emulsion of polytetrafluoroethylene (A) with a number average molecular weight of 5×106 or more and an emulsion of polytetrafluoroethylene (B) with a number average molecular weight of 1×106 to 4×106 so that the solid content ratio (A/B) of the polytetrafluoroethylene (A) and the polytetrafluoroethylene (B) is 99/1 to 10/90 is subjected to compression molding in a melted state under a reduced-pressure atmosphere to obtain a film and
(II) a step in which said film is melt stretched,
wherein said melt stretching is biaxial stretching,
said step (I) has a step (I-1) in which said resin composition is pressed at the first pressure V1 (0.01-100 MPa) for 1-100 minutes in a state where it has been heated to a temperature T1 (15-150° C.) under a reduced-pressure atmosphere, and a step (I-2) in which the heated and pressed resin composition in said step (I-1) is further heated at a temperature T2 (330-420° C.) to a melted state, and compression molded at second pressure V2 (0.01-100 MPa) for 1-100 minutes under a reduced-pressure atmosphere,
said reduced-pressure atmosphere in said steps (I) and (II) is 10 Torr or less, and
the difference of said second pressure V2 and said first pressure V1 (V2−V1) ranges between about 0 0.1-99 MPa., and
in which haze is 45% or less, and tensile strength at break is 30 MPa or more.