# US 2013/0156632 A1 · Process for making silver powder particles with small size crystallites

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2013/0156632 A1
- Document ID: US20130156632A1
- Status: Published application
- Kind: A1
- Application number: 13/406,900
- Filed: 2012-02-28
- Published: 2013-06-20
- Earliest claimed: 2011-03-08
- Assignees: E. I. Du Pont de Nemours and Company
- Inventors: ROBERTO IRIZARRY; Haixin Yang
- Web page: https://patentgrep.com/patent/US20130156632A1

## CPC

- B22F 9/24: starting from liquid metal compounds, e.g. solutions
- B22F 1/05: Metallic powder characterised by the size or surface area of the particles
- B22F 1/07: Metallic powder characterised by particles having a nanoscale microstructure (nanosized particles B22F1/054)
- C22C 5/06: Alloys based on silver
- C23C 24/087: {Coating with metal alloys or metal elements only}
- H01B 1/02: mainly consisting of metals or alloys
- H10F 77/211: {for photovoltaic cells}
- B22F 2301/255: Silver or gold
- B22F 2304/10: Micron size particles, i.e. above 1 micrometer up to 500 micrometer
- Y02E 10/50: Photovoltaic [PV] energy
- B22F: WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER (making alloys by powder metallurgy C22C); APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- H01B: CABLES; CONDUCTORS; INSULATORS; SELECTION OF MATERIALS FOR THEIR CONDUCTIVE, INSULATING OR DIELECTRIC PROPERTIES (selection for magnetic properties H01F1/00; waveguides H01P {; printed circuits H05K})
- H10F: INORGANIC SEMICONDUCTOR DEVICES SENSITIVE TO INFRARED RADIATION, LIGHT, ELECTROMAGNETIC RADIATION OF SHORTER WAVELENGTH OR CORPUSCULAR RADIATION
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

The process for making silver powder particles with small size crystallites uses a combination of gum arabic and maleic acid with the reduction of a silver salt with ascorbic acid. Silver thick film paste containing these silver powder particles can be used in electronic applications to form electrodes for semiconductor devices and, in particular, solar cells.

## Claims

### Claim 1

A process for making silver powder particles, said process comprising:
(a) preparing an acidic aqueous silver salt solution comprising a water soluble silver salt dissolved in deionized water;
(b) preparing an acidic aqueous reducing and particle modifier solution comprising:
(i) a reducing agent selected from the group consisting of ascorbic acid, ascorbates and mixtures thereof dissolved in deionized water;
(ii) nitric acid;
(iii) gum arabic;
(iv) maleic acid; and
(v) deionized water;
(c) maintaining said acidic aqueous silver salt solution and said acidic reducing and particle modifier solution at the same temperature, wherein said temperature is in the range of 10° C. to 65° C., while stirring each said solution during and after preparation;
(d) adding said acidic aqueous silver salt solution to said acidic aqueous reducing and particle modifier solution while stirring to make a reaction mixture and maintaining the temperature of said reaction mixture at said temperature of (c), wherein said silver powder particles precipitate and are contained within the resulting final aqueous solution; and
(e) increasing the temperature of said final aqueous solution to a temperature in the range of 65° C. to 80° C. while continuing stirring;
said silver powder particles comprising crystallites between 30 and 47 nm in size as determined by X-ray diffraction and the Scherrer formula; and
said silver powder particles having d50 in the range of 0.5 to 3.5 μm.

### Claim 2 (depends on 1)

The process of claim 1, further comprising:
(f) separating said silver powder particles from said final aqueous solution;
(g) washing said silver powder particles with deionized water; and
(h) drying said silver powder particles.

### Claim 3 (depends on 1)

The process of claim 1, wherein said water soluble silver salt is silver nitrate.

### Claim 4 (depends on 1)

The process of claim 1, wherein said reducing agent is ascorbic acid.

### Claim 5 (depends on 1)

The process of claim 1, said acidic aqueous reducing and particle modifier solution further comprising a metal colloid selected from the group consisting of gold colloid and silver colloid.

### Claim 6 (depends on 5)

The process of claim 5, wherein said metal colloid is gold colloid.

### Claim 7 (depends on 1)

The process of claim 1, wherein the temperature in step (c) is in the range of 10° C. to 35° C. and the temperature in step (e) is in the range of 65° C. to 75° C.

### Claim 8 (depends on 7)

The process of claim 7, wherein the temperature in step (c) is 25° C. and the temperature in step (e) is 70° C.

### Claim 9 (depends on 1)

The process of claim 1, wherein said silver powder particles have a size distribution such that (d90−d10)/d50<2.2.

### Claim 10 (depends on 1)

The process of claim 1, wherein said silver powder particles have a solids content in excess of 99% as determined by thermogravimetric analysis.

### Claim 11 (depends on 1)

The process of claim 1, wherein said silver powder particles have a TMA shrinkage of at least −10%.

### Claim 12 (depends on 1)

The process of claim 1, wherein said crystallites are between 30 and 39 nm in size.

### Claim 13 (depends on 1)

The silver powder particles made by the process of claim 1

### Claim 14 (depends on 13)

A silver thick film paste comprising said silver powder particles of claim 13.

### Claim 15 (depends on 14)

A semiconductor device comprising an electrode, said electrode, prior to firing, comprising said silver thick film paste of claim 14.

### Claim 16 (depends on 14)

A solar cell comprising an electrode, said electrode, prior to firing, comprising said silver thick film paste of claim 14.