# US 2013/0153096 A1 · High-yield-ratio and high-strength steel sheet excellent in workability

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2013/0153096 A1
- Document ID: US20130153096A1
- Status: Published application
- Kind: A1
- Application number: 13/690,552
- Filed: 2012-11-30
- Published: 2013-06-20
- Earliest claimed: 2011-12-19
- Assignees: Kabushiki Kaisha Kobe Seiko Sho (Kobe Steel, Ltd.)
- Inventors: Kazuyuki HAMADA; Tatsuya ASAI
- Web page: https://patentgrep.com/patent/US20130153096A1

## CPC

- C21D 8/0263: {following hot rolling}
- C21D 6/005: {containing Mn}
- C21D 8/0226: {Hot rolling}
- C21D 8/0236: {Cold rolling}
- C21D 8/0247: characterised by the heat treatment
- C21D 9/46: for sheet metals
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- C22C 38/22: with molybdenum or tungsten
- C22C 38/24: with vanadium
- C22C 38/26: with niobium or tantalum
- C22C 38/28: with titanium or zirconium
- C22C 38/32: with boron
- C22C 38/38: with more than 1.5% by weight of manganese
- C21D 2211/002: Bainite
- C21D 2211/005: Ferrite
- C21D 2211/008: Martensite
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

Provided is a steel sheet having a tensile strength of 980 MPa or more and exhibiting a high yield ratio and an excellent workability. The steel sheet includes C, Si, Mn, B, at least one of Ti, Nb and V, P, S, Al and N, the content by percentage of each of which is in a specified range. The metal structure thereof includes bainite, and martensite and may include ferrite. The proportion by area of bainite in the entire metal structure is 42 to 85%, that of martensite is 15 to 50%, that of ferrite is 5% or less, and that of entire microstructure of the balance other than bainite, martensite and ferrite is 3% or less thereof. Furthermore, bainite has an average crystal grain diameter of 7 μm or less.

## Claims

### Claim 1

A steel sheet, which has a chemical composition comprising:
C: 0.05% or more and less than 0.12% provided that the “%”s each mean “% by mass” and hereinafter the same matter is applied to any “%” described in connection with the chemical composition,
Si: 0.1% or less, which is not 0%,
Mn: 2.0 to 3.5%,
at least one selected from the group consisting of Ti, Nb, and V: 0.01 to 0.2% in total,
B: 0.0003 to 0.005%,
P: 0.05% or less,
S: 0.05% or less,
Al: 0.1% or less,
N: 0.015% or less, and
Fe and one or more inevitable impurities as the balance of the composition;
which has a metal structure comprising:
bainite: 42 to 85%,
martensite: 15 to 50%,
ferrite: 5% or less, and
entire microstructure of the balance of the metal structure other than bainite, martensite and ferrite: 3% or less provided that these proportions are each the proportion by area of one of these microstructures in the whole of the metal structure, and further satisfying a requirement that bainite has an average crystal grain diameter of 7 μm or less; and
which has a tensile strength of 980 MPa or more.

### Claim 2 (depends on 1)

The steel sheet of claim 1,
wherein Cr and Mo are comprised in a total content by percentage of 1.0% or less.

### Claim 3 (depends on 1)

A method for manufacturing the steel sheet of claim 1, comprising the following steps to be conducted in the description order thereof:
the step of preparing a steel having the composition recited in claim 1;
a soaking step of subjecting the steel to hot rolling and cold rolling, and then keeping the steel at a temperature ranging from the Ac3 point of the steel to a temperature of (the Ac3 point+150° C.) for 5 to 200 seconds;
a cooling step of cooling the steel at an average cooling rate of 5° C./second, or more; and
a low-temperature-keeping step of keeping the steel at a temperature ranging from the Ms point of the steel to a temperature of (the Ms point+50° C.) for 15 to 600 seconds.