# US 2013/0153091 A1 · Hot-rolled steel sheet, cold-rolled steel sheet, galvanized steel sheet, and methods of manufacturing the same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2013/0153091 A1
- Document ID: US20130153091A1
- Status: Published application
- Kind: A1
- Application number: 13/811,902
- Filed: 2011-07-27
- Published: 2013-06-20
- Earliest claimed: 2010-07-28
- Assignees: Nippon Steel & Sumitomo Metal Corporation
- Inventors: Nobuhiro Fujita; Kunio Hayashi; Riki Okamoto; Manabu Takahashi; Tetsuo Kishimoto; Hiroshi Yoshida
- Web page: https://patentgrep.com/patent/US20130153091A1

## CPC

- C25D 3/22: of zinc
- B21B 35/00: Drives for metal-rolling mills {, e.g. hydraulic drives}
- B32B 15/013: {one layer being formed of an iron alloy or steel, another layer being formed of a metal other than iron or aluminium}
- C21D 6/004: {containing Cr and Ni}
- C21D 6/005: {containing Mn}
- C21D 6/007: {containing Co}
- C21D 6/008: {containing Si}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0226: {Hot rolling}
- C21D 8/0236: {Cold rolling}
- C21D 8/0247: characterised by the heat treatment
- C21D 8/0263: {following hot rolling}
- C21D 8/0273: {Final recrystallisation annealing}
- C21D 9/46: for sheet metals
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/004: {Very low carbon steels, i.e. having a carbon content of less than 0,01%}
- C22C 38/005: {containing rare earths, i.e. Sc, Y, Lanthanides}
- C22C 38/008: {containing tin}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/08: containing nickel {(C22C38/105 takes precedence)}
- C22C 38/10: containing cobalt
- C22C 38/105: {containing Co and Ni}
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- C22C 38/16: containing copper
- C22C 38/18: containing chromium
- C22C 38/20: with copper
- C22C 38/22: with molybdenum or tungsten
- C22C 38/24: with vanadium
- C22C 38/26: with niobium or tantalum
- C22C 38/28: with titanium or zirconium
- C22C 38/30: with cobalt
- C22C 38/32: with boron
- C22C 38/34: with more than 1.5% by weight of silicon
- C22C 38/38: with more than 1.5% by weight of manganese
- C22C 38/40: with nickel
- C22C 38/42: with copper
- C22C 38/44: with molybdenum or tungsten
- C22C 38/46: with vanadium
- C22C 38/48: with niobium or tantalum
- C22C 38/50: with titanium or zirconium
- C22C 38/52: with cobalt
- C22C 38/54: with boron
- C22C 38/58: with more than 1.5% by weight of manganese
- C23C 2/02: Pretreatment of the material to be coated, e.g. for coating on selected surface areas (C23C2/30 takes precedence)
- C23C 2/0224: {Two or more thermal pretreatments}
- C23C 2/024: {by cleaning or etching}
- C23C 2/06: Zinc or cadmium or alloys based thereon
- C23C 2/40: Plates; Strips
- C25D 5/36: of iron or steel
- C21D 2201/05: Grain orientation
- C21D 2211/00: Microstructure comprising significant phases
- C21D 2211/001: Austenite
- C21D 2211/002: Bainite
- C21D 2211/005: Ferrite
- C21D 2211/009: Pearlite
- C25D: PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR
- B21B: ROLLING OF METAL (auxiliary operations used in connection with metal-working operations covered in B21, see B21C; bending by rolling B21D; manufacture of particular objects, e.g. screws, wheels, rings, barrels, balls, by rolling B21H; pressure welding by means of a rolling mill B23K20/04)
- B32B: LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)

## Abstract

A hot-rolled steel sheet has an average value of the X-ray random intensity ratio of a {100} <011> to {223} <110> orientation group at least in a sheet thickness central portion that is in a sheet thickness range of ⅝ to ⅜ from a steel sheet surface of 1.0 to 6.0, an X-ray random intensity ratio of a {332} <113> crystal orientation of 1.0 to 5.0, rC which is an r value in a direction perpendicular to a rolling direction of 0.70 to 1.10, and r30 which is an r value in a direction that forms an angle of 30° with respect to the rolling direction of 0.70 to 1.10.

## Claims

### Claim 1

A hot-rolled steel sheet comprising, by mass %:
C: 0.0001% to 0.40%;
Si: 0.001% to 2.5%;
Mn: 0.001% to 4.0%;
P: 0.001% to 0.15%;
S: 0.0005% to 0.03%;
Al: 0.001% to 2.0%;
N: 0.0005% to 0.01%;
O: 0.0005% to 0.01%;
and further comprising one or two or more of:
Ti: 0.001% to 0.20%;
Nb: 0.001% to 0.20%;
V: 0.001% to 1.0%;
W: 0.001% to 1.0%;
B: 0.0001% to 0.0050%;
Mo: 0.001% to 1.0%;
Cr: 0.001% to 2.0%;
Cu: 0.001% to 2.0%;
Ni: 0.001% to 2.0%;
Co: 0.0001% to 1.0%;
Sn: 0.0001% to 0.2%;
Zr: 0.0001% to 0.2%;
As: 0.0001% to 0.50%;
Mg: 0.0001% to 0.010%;
Ca: 0.0001% to 0.010%; and
REM: 0.0001% to 0.1%;
and balance composed of iron and inevitable impurities,
wherein an average value of an X-ray random intensity ratio of a {100} <011> to {223}<110> orientation group at least in a sheet thickness central portion that is in a sheet thickness range of ⅝ to ⅜ from a steel sheet surface is 1.0 to 6.0, an X-ray random intensity ratio of a {332} <113> crystal orientation is 1.0 to 5.0; and
rC which is an r value in a direction perpendicular to a rolling direction is 0.70 to 1.10, and r30 which is an r value in a direction that forms an angle of 30° with respect to the rolling direction is 0.70 to 1.10.

### Claim 2 (depends on 1)

The hot-rolled steel sheet according to claim 1,
wherein rL which is an r value in the rolling direction is 0.70 to 1.10, and r60 which is an r value in a direction that forms an angle of 60° with respect to the rolling direction is 0.70 to 1.10.

### Claim 3 (depends on 1)

The hot-rolled steel sheet according to claim 1,
wherein one or two or more of bainite, martensite, pearlite, and austenite are present in the hot-rolled steel sheet, and a proportion of grains having a dL/dt, which is a ratio of a length in the rolling direction dL to a length of a sheet thickness direction dt, of 3.0 or less in crystal grains in the structures is 50% to 100%.

### Claim 4 (depends on 1)

The hot-rolled steel sheet according to claim 1,
wherein an area proportion of crystal grains having a grain diameter of more than 20 μm in a total area of a metallic structure in the hot-rolled steel sheet is 0% to 10%.

### Claim 5 (depends on 1)

A cold-rolled steel sheet obtained through cold rolling of the hot-rolled steel sheet according to claim 1,
wherein the average value of the X-ray random intensity ratio of the {100} <011> to {223} <110> orientation group at least in the sheet thickness central portion is 1.0 to less than 4.0, the X-ray random intensity ratio of the {332} <113> crystal orientation is 1.0 to 5.0; and
rC which is the r value in a direction perpendicular to the rolling direction is 0.70 to 1.10, and r30 which is the r value in a direction that forms an angle of 30° with respect to the rolling direction is 0.70 to 1.10.

### Claim 6 (depends on 5)

The cold-rolled steel sheet according to claim 5,
wherein rL which is an r value in the rolling direction is 0.70 to 1.10, and r60 which is an r value in a direction that forms an angle of 60° with respect to the rolling direction is 0.70 to 1.10.

### Claim 7 (depends on 5)

The cold-rolled steel sheet according to claim 5,
wherein one or two or more of bainite, martensite, pearlite, and austenite are present in the cold-rolled steel sheet, and a proportion of grains having a dL/dt, which is a ratio of a length in the rolling direction dL to a length of a sheet thickness direction dt, of 3.0 or less in crystal grains in the structures is 50% to 100%.

### Claim 8 (depends on 5)

The cold-rolled steel sheet according to claim 5,
wherein an area proportion of crystal grains having a grain diameter of more than 20 μm in a total area of a metallic structure in the cold-rolled steel sheet is 0% to 10%.

### Claim 9 (depends on 5)

A galvanized steel sheet further comprising a galvanized coating layer or a galvanealed coating layer on a surface of the cold-rolled steel sheet according to claim 5,
wherein the average value of the X-ray random intensity ratio of the {100} <011> to {223} <110> orientation group at least in the sheet thickness central portion is 1.0 to less than 4.0, the X-ray random intensity ratio of the {332} <113> crystal orientation is 1.0 to 5.0; and
rC which is the r value in a direction perpendicular to the rolling direction is 0.70 to 1.10, and r30 which is the r value in a direction that forms an angle of 30° with respect to the rolling direction is 0.70 to 1.10.

### Claim 10 (depends on 9)

The galvanized steel sheet according to claim 9,
wherein rL which is an r value in the rolling direction is 0.70 to 1.10, and r60 which is an r value in a direction that forms an angle of 60° with respect to the rolling direction is 0.70 to 1.10.

### Claim 11

A method of manufacturing the hot-rolled steel sheet, the method comprising,
first hot rolling carried out at least once at a rolling reduction ratio of 20% or more in a temperature range of 1000° C. to 1200° C., and an austenite grain diameter is set to 200 μM or less, wherein
an ingot or slab containing, by mass %:
C: 0.0001% to 0.40%,
Si: 0.001% to 2.5%,
Mn: 0.001% to 4.0%,
P: 0.001% to 0.15%,
S: 0.0005% to 0.03%,
Al: 0.001% to 2.0%,
N: 0.0005% to 0.01%,
O: 0.0005% to 0.01%,
and further comprising one or two or more of:
Ti: 0.001% to 0.20%,
Nb: 0.001% to 0.20%,
V: 0.001% to 1.0%,
W: 0.001% to 1.0%,
B: 0.0001% to 0.0050%,
Mo: 0.001% to 1.0%,
Cr: 0.001% to 2.0%;
Cu: 0.001% to 2.0%,
Ni: 0.001% to 2.0%,
Co: 0.0001% to 1.0%,
Sn: 0.0001% to 0.2%,
Zr: 0.0001% to 0.2%,
As: 0.0001% to 0.50%,
Mg: 0.0001% to 0.010%,
Ca: 0.0001% to 0.010%, and
REM: 0.0001% to 0.1%
and balance composed of iron and inevitable impurities;
second hot rolling in which a total of rolling reduction ratios is 50% or more is carried out in a temperature range of T1+30° C. to T1+200° C.;
third hot rolling in which a total of rolling reduction ratios is less than 30% is carried out in a temperature range of T1° C. to lower than T1+30° C.; and
hot rolling ends at an Ar3 transformation temperature or higher,
where, T1 is a temperature determined by steel sheet components, and expressed by the following formula 1,
T1(° C.)=850+10×(C+N)×Mn+350×Nb+250×Ti+40×B+10×Cr+100×Mo+100×V (Formula 1).

### Claim 12 (depends on 11)

The method of manufacturing a hot-rolled steel sheet according to claim 11,
wherein, in the second hot rolling in the temperature range of T1+30° C. to T1+200° C., the ingot or slab is rolled at least once at a rolling reduction ratio of 30% or more in a pass.

### Claim 13 (depends on 11)

The method of manufacturing a hot-rolled steel sheet according to claim 11,
wherein, in the first hot rolling in a temperature range of 1000° C. to 1200° C., the ingot or slab is rolled at least twice at a rolling reduction ratio of 20% or more, and the austenite grain diameter is set to 100 μm or less.

### Claim 14 (depends on 11)

The method of manufacturing a hot-rolled steel sheet according to claim 11,
wherein, in a case in which the pass in which the rolling reduction ratio is 30% or more in the temperature range of T1+30° C. to T1+200° C. is defined as a large reduction pass, a waiting time t from completion of a final pass of the large reduction pass to initiation of cooling employs a configuration that satisfies the following formula 2,
t1≦t≦t1×2.5 (Formula 2)
where t1 is expressed by the following formula 3;
t1=0.001×((Tf−T1)×P1)2−0.109×((Tf−T1)×P1)+3.1 (Formula 3)
where Tf represents a temperature after the final pass, and P1 represents a rolling reduction ratio in the final pass.

### Claim 15 (depends on 14)

The method of manufacturing a hot-rolled steel sheet according to claim 14,
wherein a temperature of the steel sheet increases by 18° C. or less between the respective passes of the second hot rolling in the temperature range of T1+30° C. to T1+200° C.

### Claim 16 (depends on 11)

A method of manufacturing a cold-rolled steel sheet, the method comprising,
pickling, after the end of the hot rolling the hot-rolled steel sheet obtained through the method of manufacturing the hot-rolled steel sheet according to claim 11 at the Ar3 transformation temperature or higher;
cold-rolling at 20% to 90%;
annealing at a temperature range of 720° C. to 900° C. for a holding time of 1 second to 300 seconds;
acceleration-cooling at a cooling rate of 10° C./s to 200° C./s from 650° C. to 500° C.; and
helding at a temperature of 200° C. to 500° C.

### Claim 17 (depends on 16)

The method of manufacturing a cold-rolled steel sheet according to claim 16,
wherein, in the second hot rolling in the temperature range of T1+30° C. to T1+200° C., rolling at a rolling reduction ratio of 30% or more in a pass is carried out at least once.

### Claim 18 (depends on 16)

The method of manufacturing a cold-rolled steel sheet according to claim 16,
wherein, in the first hot rolling in the temperature range of 1000° C. to 1200° C., rolling at a rolling reduction ratio of 20% or more is carried out at least twice, and the austenite grain diameter is set to 100 μm or less.

### Claim 19 (depends on 16)

The method of manufacturing a cold-rolled steel sheet according to claim 16,
wherein, in a case in which the pass in which the rolling reduction ratio is 30% or more in the temperature range of T1+30° C. to T1+200° C. is defined as a large reduction pass, a waiting time t from completion of a final pass of the large reduction pass to initiation of cooling employs a configuration that satisfies the following formula 4,
t1≦t≦t1×2.5 (Formula 4)
where t1 is expressed by the following formula 5;
t1=0.001×((Tf−T1)×P1)2−0.109×((Tf−T1)×P1)+3.1 (Formula 5)
where Tf represents a temperature after the final pass, and P1 represents a rolling reduction ratio in the final pass.

### Claim 20 (depends on 19)

The method of manufacturing a cold-rolled steel sheet according to claim 19,
wherein a temperature of the steel sheet increases by 18° C. or less between the respective passes of the second hot rolling in the temperature range of T1+30° C. to T1+200° C.

### Claim 21 (depends on 11)

A method of manufacturing a galvanized steel sheet, the method comprising,
a winding in a temperature range of 680° C. to room temperature, after the end of the hot rolling the hot-rolled steel sheet obtained through the method of manufacturing the hot-rolled steel sheet according to claim 11 at the Ar3 transformation temperature or higher;
pickling;
cold-rolling at 20% to 90%;
heating to a temperature range of 650° C. to 900° C.;
annealing for a holding time of 1 second to 300 seconds;
cooling at a cooling rate of 0.1° C./s to 100° C./s from 720° C. to 580° C.; and
galvanizing treating.

### Claim 22 (depends on 21)

The method of manufacturing a galvanized steel sheet according to claim 21,
wherein, in the second hot rolling in the temperature range of T1+30° C. to T1+200° C., rolling at a rolling reduction ratio of 30% or more in a pass is carried out at least once.

### Claim 23 (depends on 21)

The method of manufacturing a galvanized steel sheet according to claim 21,
wherein, in the first hot rolling in the temperature range of 1000° C. to 1200° C., rolling at a rolling reduction ratio of 20% or more is carried out at least twice, and the austenite grain diameter is set to 100 μm or less.

### Claim 24 (depends on 21)

The method of manufacturing a galvanized steel sheet according to claim 21,
wherein, in a case in which the pass in which the rolling reduction ratio is 30% or more in the temperature range of T1+30° C. to T1+200° C. is defined as a large reduction pass, a waiting time t from completion of a final pass of the large reduction pass to initiation of cooling employs a configuration that satisfies the following formula 6,
t1≦t≦t1×2.5 (Formula 6)
where t1 is expressed by the following formula 7;
t1=0.001×((Tf−T1)×P1)2−0.109×((Tf−T1)×P1)+3.1 (Formula 7)
where Tf represents a temperature after the final pass, and P1 represents a rolling reduction ratio in the final pass.

### Claim 25 (depends on 24)

The method of manufacturing a galvanized steel sheet according to claim 24,
wherein a temperature of the steel sheet increases by 18° C. or less between the respective passes of the second hot rolling in the temperature range of T1+30° C. to T1+200° C.