# US 2013/0094900 A1 · Hardfacing alloy, methods, and products thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2013/0094900 A1
- Document ID: US20130094900A1
- Status: Published application
- Kind: A1
- Application number: 13/275,023
- Filed: 2011-10-17
- Published: 2013-04-18
- Earliest claimed: 2011-10-17
- Assignees: Devasco International Inc.
- Inventors: Grant R. FOLKMANN; Keith E. MOLINE
- Web page: https://patentgrep.com/patent/US20130094900A1

## CPC

- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- B23K 9/048: {on cylindrical surfaces}
- B23K 9/173: and of a consumable electrode
- B23K 9/23: taking account of the properties of the materials to be welded
- B32B 15/01: all layers being exclusively metallic {(making layered metal workpieces by pressure cladding B23K20/22; making coatings with a metallic material characterised by its composition C23C30/00)}
- C22C 33/0257: {characterised by the range of the alloying elements}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C23C 4/04: characterised by the coating material
- C23C 30/00: Coating with metallic material characterised only by the composition of the metallic material, i.e. not characterised by the coating process (C23C26/00, C23C28/00 take precedence)
- B23K 2101/10: Pipe-lines
- B23K 2103/04: Steel {or steel} alloys
- B23K 2103/05: {Stainless steel}
- Y10T 428/12222: Shaped configuration for melting [e.g., package, etc.]
- Y10T 428/12653: Fe, containing 0.01-1.7% carbon [i.e., steel]
- Y10T 428/12778: Alternative base metals from diverse categories
- Y10T 428/12972: Containing 0.01-1.7% carbon [i.e., steel]
- Y10T 428/12979: Containing more than 10% nonferrous elements [e.g., high alloy, stainless]
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- B23K: SOLDERING OR UNSOLDERING; WELDING; CLADDING OR PLATING BY SOLDERING OR WELDING; CUTTING BY APPLYING HEAT LOCALLY, e.g. FLAME CUTTING; WORKING BY LASER BEAM
- B32B: LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- Y10T: TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION

## Abstract

Disclosed is a hardfacing alloy deriving its usefulness from carbides and borides of molybdenum and niobium. The alloy does not rely on chromium as an alloying agent. The hardfacing alloy is capable of being applied to a number of industrial substrates in a crack-free manner, and once applied convert the substrate to a wear- and abrasion-resistant material having an extended service life, even when subjected to harsh wear conditions.

## Claims

### Claim 1

An alloy composition comprising:
from about 0.0 weight percent to about 5.0 weight percent carbon;
from about 2.5 weight percent to about 8.0 weight percent molybdenum;
from about 2.5 weight percent to about 8.0 weight percent niobium;
from about 0.0 weight percent to about 3.0 weight percent boron; and
the balance of the composition being iron, including impurities in trace amounts.

### Claim 2 (depends on 1)

The alloy of claim 1, wherein the composition comprises:
from about 0.3 weight percent to about 3.0 weight percent carbon;
from about 3.0 weight percent to about 6.0 weight percent molybdenum;
from about 3.0 weight percent to about 6.0 weight percent niobium;
from about 0.5 weight percent to about 5.0 weight percent manganese;
from about 0.0 weight percent to about 2.0 weight percent boron; and
from about 0.0 weight percent to about 3.0 weight percent silicon,
the balance of the composition being iron, including impurities in trace amounts.

### Claim 3 (depends on 1)

The alloy of claim 1, wherein the composition comprises:
from about 1.0 weight percent to about 2.0 weight percent carbon;
from about 4.0 weight percent to about 6.0 weight percent molybdenum;
from about 4.0 weight percent to about 6.0 weight percent niobium;
from about 0.5 weight percent to about 3.5 weight percent manganese;
from about 0.5 weight percent to about 1.5 weight percent boron; and
from about 0.5 weight percent to about 2.0 weight percent silicon,
the balance of the composition being iron, including impurities in trace amounts.

### Claim 4 (depends on 1)

The alloy of claim 1, wherein the composition comprises:
from about 1.0 weight percent to about 2.0 weight percent carbon;
from about 4.5 weight percent to about 6.5 weight percent molybdenum;
from about 4.5 weight percent to about 6.5 weight percent niobium;
from about 1.0 weight percent to about 3.5 weight percent manganese;
from about 0.5 weight percent to about 1.5 weight percent boron; and
from about 0.5 weight percent to about 2.0 weight percent silicon,
the balance of the composition being iron, including impurities in trace amounts.

### Claim 6 (depends on 1)

The alloy composition of claim 1, wherein the molybdenum and the niobium are in approximately equal amounts.

### Claim 7 (depends on 1)

The alloy of claim 1, wherein the alloy is contained in a metal core tubular wire.

### Claim 8 (depends on 1)

The alloy of claim 1, wherein the alloy exhibits a hardness on the Rockwell-C Hardness scale of from about 55 Rc to about 67 Rc, inclusive.

### Claim 9 (depends on 1)

The alloy of claim 1, wherein the alloy, deposited in a single or double layer upon a tool joint, exhibits a wear rate from about 0.175 g to about 0.275 g weight loss per 6,000 revolutions as determined using ASTM test method G-65.

### Claim 10 (depends on 1)

The alloy of claim 1, wherein the alloy is deposited on the surface of a substrate in a crack-free manner.

### Claim 11

An alloy composition comprising:
from about 0.0 weight percent to about 5.0 weight percent carbon;
from about 2.5 weight percent to about 8.0 weight percent molybdenum;
from about 2.5 weight percent to about 8.0 weight percent niobium;
from about 0.0 weight percent to about 5.0 weight percent manganese;
from about 0.0 weight percent to about 3.0 weight percent boron; and
from about 0.0 weight percent to about 3.0 weight percent silicon,
the balance of the composition being iron, including impurities in trace amounts.

### Claim 12 (depends on 11)

The alloy of claim 11, wherein the composition comprises:
from about 0.3 weight percent to about 3.0 weight percent carbon;
from about 4.0 weight percent to about 6.0 weight percent molybdenum;
from about 4.0 weight percent to about 6.0 weight percent niobium;
from about 0.5 weight percent to about 5.0 weight percent manganese;
from about 0.0 weight percent to about 2.0 weight percent boron; and
from about 0.0 weight percent to about 3.0 weight percent silicon,
the balance of the composition being iron, including impurities in trace amounts.

### Claim 13 (depends on 11)

The alloy of claim 11, wherein the composition comprises:
from about 1.0 weight percent to about 2.0 weight percent carbon;
from about 4.0 weight percent to about 6.0 weight percent molybdenum;
from about 4.0 weight percent to about 6.0 weight percent niobium;
from about 0.5 weight percent to about 3.5 weight percent manganese;
from about 0.5 weight percent to about 1.5 weight percent boron; and
from about 0.5 weight percent to about 2.0 weight percent silicon,
the balance of the composition being iron, including impurities in trace amounts.

### Claim 14 (depends on 11)

The alloy of claim 11, wherein the composition comprises:
from about 1.0 weight percent to about 2.0 weight percent carbon;
from about 4.5 weight percent to about 6.5 weight percent molybdenum;
from about 4.5 weight percent to about 6.5 weight percent niobium;
from about 1.0 weight percent to about 3.5 weight percent manganese;
from about 0.5 weight percent to about 1.5 weight percent boron; and
from about 0.5 weight percent to about 2.0 weight percent silicon,
the balance of the composition being iron, including impurities in trace amounts.

### Claim 16 (depends on 11)

The alloy composition of claim 11, wherein the molybdenum and the niobium are in approximately equal amounts.

### Claim 17 (depends on 11)

The alloy of claim 11, wherein the alloy is contained in a metal core tubular wire.

### Claim 18 (depends on 11)

The alloy of claim 11, wherein the alloy exhibits a hardness on the Rockwell-C Hardness scale of from about 55 Rc to about 67 Rc, inclusive.

### Claim 19 (depends on 11)

The alloy of claim 11, wherein the alloy, deposited in a single or double layer upon a tool joint, exhibits a wear rate from about 0.175 g to about 0.275 g weight loss per 6,000 revolutions as determined using ASTM test method G-65.

### Claim 20 (depends on 11)

The alloy of claim 11, wherein the alloy is deposited on the surface of a substrate in a crack-free manner.

### Claim 21

A method of enhancing an industrial substrate, the method comprising:
selecting a substrate; and
applying an alloy onto at least a portion of a surface of the substrate, the alloy comprising:
from about 0.0 weight percent to about 5.0 weight percent carbon;
from about 2.5 weight percent to about 8.0 weight percent molybdenum;
from about 2.5 weight percent to about 8.0 weight percent niobium;
from about 0.0 weight percent to about 5.0 weight percent manganese;
from about 0.0 weight percent to about 3.0 weight percent boron; and
from about 0.0 weight percent to about 3.0 weight percent silicon,
the balance of the composition being iron, including impurities in trace amounts,
the alloy exhibiting a hardness on the Rockwell-C Hardness scale of from about 55 Rc to about 67 Rc, inclusive.

### Claim 22 (depends on 21)

The method of claim 21, wherein the application of the alloy onto the substrate comprises electric arc welding.

### Claim 23 (depends on 21)

The method of claim 21, wherein the application of the alloy onto the substrate comprises electric arc welding with a shielding gas.

### Claim 24 (depends on 21)

The method of claim 21, wherein the application of the alloy onto the substrate comprises thermal spraying.

### Claim 25 (depends on 21)

The method of claim 21, wherein the substrate is a metallic material selected from the group consisting of steel, stainless steel, iron base alloys, nickel, nickel base alloys, cobalt, cobalt base alloys, chromium, chromium base alloys, titanium, titanium base alloys, aluminum, aluminum base alloys, copper, copper base alloys, refractory metals, and refractory-metal alloys.

### Claim 26 (depends on 21)

The method of claim 21, wherein the substrate comprises a tool joint.

### Claim 27 (depends on 21)

The method of claim 21, wherein the alloy comprises:
from about 0.3 weight percent to about 5.0 weight percent carbon;
from about 4.0 weight percent to about 6.5 weight percent molybdenum;
from about 4.0 weight percent to about 6.5 weight percent niobium;
from about 0.0 weight percent to about 5.0 weight percent manganese;
from about 0.0 weight percent to about 2.0 weight percent boron; and
from about 0.0 weight percent to about 3.0 weight percent silicon,
the balance of the composition being iron, including impurities in trace amounts.

### Claim 28 (depends on 21)

The method of claim 21, wherein the alloy comprises:
from about 1.0 weight percent to about 3.0 weight percent carbon;
from about 4.0 weight percent to about 6.0 weight percent molybdenum;
from about 4.0 weight percent to about 6.0 weight percent niobium;
from about 0.5 weight percent to about 3.5 weight percent manganese;
from about 0.5 weight percent to about 1.5 weight percent boron; and
from about 0.5 weight percent to about 2.0 weight percent silicon,
the balance of the composition being iron, including impurities in trace amounts.

### Claim 29 (depends on 21)

The method of claim 21, wherein the alloy comprises:
from about 1.0 weight percent to about 2.0 weight percent carbon;
from about 4.5 weight percent to about 6.5 weight percent molybdenum;
from about 4.5 weight percent to about 6.5 weight percent niobium;
from about 1.0 weight percent to about 3.5 weight percent manganese;
from about 0.5 weight percent to about 1.5 weight percent boron; and
from about 0.5 weight percent to about 2.0 weight percent silicon,
the balance of the composition being iron, including impurities in trace amounts.

### Claim 31 (depends on 21)

The method of claim 21, wherein the molybdenum and the niobium in the alloy composition are present in approximately equal amounts.

### Claim 32 (depends on 21)

The method of claim 21, further comprising increasing a wear resistance of the substrate material while simultaneously providing a lower coefficient of friction of the alloy layer relative to a coefficient of friction of the substrate without the alloy.

### Claim 33 (depends on 21)

The method of claim 21, wherein the method presents a substrate having a wear rate from about 0.175 g to about 0.275 g weight loss per 6,000 revolutions as determined using ASTM test method G-65.

### Claim 34

A powdered admixture comprising:
from about 0.0 weight percent to about 5.0 weight percent carbon;
from about 2.5 weight percent to about 8.0 weight percent molybdenum;
from about 2.5 weight percent to about 8.0 weight percent niobium;
from about 0.0 weight percent to about 5.0 weight percent manganese;
from about 0.0 weight percent to about 3.0 weight percent boron; and
from about 0.0 weight percent to about 3.0 weight percent silicon,
the balance of the composition being iron, including impurities in trace amounts.

### Claim 35 (depends on 34)

The powdered admixture of claim 34, comprising:
from about 0.3 weight percent to about 3.0 weight percent carbon;
from about 4.0 weight percent to about 6.5 weight percent molybdenum;
from about 4.0 weight percent to about 6.5 weight percent niobium;
from about 0.0 weight percent to about 5.0 weight percent manganese;
from about 0.0 weight percent to about 2.0 weight percent boron; and
from about 0.0 weight percent to about 3.0 weight percent silicon,
the balance of the composition being iron, including impurities in trace amounts

### Claim 36 (depends on 34)

The powdered admixture of claim 34, comprising:
from about 1.0 weight percent to about 2.0 weight percent carbon;
from about 4.0 weight percent to about 6.5 weight percent molybdenum;
from about 4.0 weight percent to about 6.5 weight percent niobium;
from about 0.5 weight percent to about 3.5 weight percent manganese;
from about 0.5 weight percent to about 1.5 weight percent boron; and
from about 0.5 weight percent to about 2.0 weight percent silicon,
the balance of the composition being iron, including impurities in trace amounts

### Claim 37 (depends on 34)

The powdered admixture of claim 34, comprising:
from about 1.0 weight percent to about 2.0 weight percent carbon;
from about 4.5 weight percent to about 6.5 weight percent molybdenum;
from about 4.5 weight percent to about 6.5 weight percent niobium;
from about 1.0 weight percent to about 3.5 weight percent manganese;
from about 0.5 weight percent to about 1.5 weight percent boron; and
from about 0.5 weight percent to about 2.0 weight percent silicon,
the balance of the composition being iron, including impurities in trace amounts

### Claim 39 (depends on 34)

The powdered admixture of claim 34, wherein the molybdenum and the niobium are in approximately equal amounts.

### Claim 40

A wear and corrosion resistant alloy on a substrate, the alloy comprising hard, ultrafine, transition metal particles dispersed in a matrix and comprising:
from about 0.0 weight percent to about 3.0 weight percent carbon;
from about 2.5 weight percent to about 8.0 weight percent molybdenum;
from about 2.5 weight percent to about 8.0 weight percent niobium;
from about 0.0 weight percent to about 2.0 weight percent boron; and
from about 0.0 weight percent to about 2.5 weight percent silicon,
the balance of the composition being iron, including impurities in trace amounts

### Claim 41 (depends on 40)

An alloy according to claim 40, comprising:
from about 0.3 weight percent to about 3.0 weight percent carbon;
from about 3.0 weight percent to about 7.0 weight percent molybdenum;
from about 3.0 weight percent to about 7.0 weight percent niobium;
from about 0.5 weight percent to about 3.5 weight percent manganese;
from about 0.5 weight percent to about 2.0 weight percent boron; and
from about 0.5 weight percent to about 2.0 weight percent silicon,
the balance of the composition being iron, including impurities in trace amounts

### Claim 42 (depends on 40)

An alloy according to claim 40, having a hardness from about 600 to about 900 DPH300 (Vickers DPH (Diamond Pyramid Hardness) hardness, HV.3.

### Claim 43 (depends on 40)

An alloy according to claim 40, having a hardness from about 55 Rc to about 67 Rc on the Rockwell-C hardness scale.

### Claim 44 (depends on 40)

An alloy according to claim 40, having a wear rate from about 0.175 g to about 0.275 g weight loss per 6,000 revolutions as determined using ASTM test method G-65.

### Claim 45

An alloy for welding to a surface to be abrasion resistant comprising by weight,
about 0.3 to about 3.0 percent carbon,
about 0.5 to about 2.0 percent boron,
about 2.5 to about 7.0 percent molybdenum,
about 2.5 to about 7.0 percent niobium,
about 0.5 to about 3.5 percent manganese,
about 0.6 to about 0.8 percent silicon,
and the balance iron, including impurities as trace elements,
the alloy having a hardness of from about 55 Rc (600 Hv) to about 67 Rc (900 Hv).

### Claim 46 (depends on 45)

An industrial product having a surface subject to abrasion comprising, a layer of the alloy of claim 45 welded to the surface of the industrial product subject to such abrasion.

### Claim 47 (depends on 45, 46)

The industrial product of claim 46 comprising, a stabilizer having a cylindrical body and an internally threaded box and an externally threaded pin for connection in a string of drill pipe, stabilizer ribs having outer surfaces subject to the abrasion extending from an outer surface of the cylindrical body effective to stabilize the string of drill pipe in a well bore, and a layer of the alloy of claim 45 welded to the outer surfaces of the stabilizer ribs subject to the abrasion.

### Claim 48 (depends on 45)

A tool joint for connecting together drill pipe, the tool joint having a cylindrical body, an internally threaded box which has an outer cylindrical surface of a diameter greater than the drill pipe, and an externally threaded pin including, at least one layer of the alloy of claim 45 welded to the outer cylindrical surface of one or both of the box or pin, thereby providing surface resistance to abrasion by silicious materials.

### Claim 49 (depends on 48)

The tool joint of claim 48 where, the outer cylindrical surface of one or both the box or pin has a reduced diameter portion extending along a substantial portion of its length, and the layer of alloy is welded to the reduced diameter portion of one or both of the box and the pin.

### Claim 50 (depends on 45)

A method of prolonging the life of an industrial product subject to abrasion of the order of silicious materials comprising, welding a layer of the alloy of claim 45 to one or more surfaces of the industrial product subject to the abrasion.

### Claim 51

An alloy composition comprising:
from about 0.0 weight percent to about 5.0 weight percent carbon;
from about 2.5 weight percent to about 8.0 weight percent molybdenum;
from about 2.5 weight percent to about 8.0 weight percent niobium;
from about 0.0 weight percent to about 3.0 weight percent boron; and
the balance of the composition being iron, including impurities in trace amounts.

### Claim 52 (depends on 51)

The alloy composition of claim 51, wherein the amount of carbon is between about 0.3 wt. % and about 3.0 wt. %.

### Claim 53 (depends on 51)

The alloy composition of claim 51, wherein the amount of molybdenum and niobium is between about 4.0 wt. % and about 6.5 wt. %.

### Claim 54 (depends on 51)

The alloy composition of claim 51, wherein the amount of boron is between about 0.5 wt. % and 1.5 wt. %.

### Claim 55 (depends on 51)

The alloy composition of claim 51, further comprising manganese in an amount between about 0.5 wt. % and 3.5 wt. %.

### Claim 56 (depends on 51)

The alloy composition of claim 51, further comprising silicon in an amount between about 0.5 wt. % and 3.5 wt. %.

### Claim 57

A hardfacing alloy for welding to a surface to be abrasion resistant comprising by weight,
about 0.3 to about 3.0 percent carbon,
about 0.5 to about 2.0 percent boron,
about 2.5 to about 7.0 percent molybdenum,
about 2.5 to about 7.0 percent niobium,
about 0.5 to about 3.5 percent manganese,
about 0.6 to about 0.8 percent silicon,
and the balance iron, including impurities as trace elements,
the alloy having a hardness of from about 55 Rc (600 Hv) to about 67 Rc (900 Hv).

### Claim 58 (depends on 57)

An industrial product having a surface subject to abrasion comprising, a layer of the hardbanding alloy of claim 57 welded to the surface of the industrial product subject to such abrasion.

### Claim 59 (depends on 57, 58)

The industrial product of claim 58 comprising, a stabilizer having a cylindrical body and an internally threaded box and an externally threaded pin for connection in a string of drill pipe, stabilizer ribs having outer surfaces subject to the abrasion extending from an outer surface of the cylindrical body effective to stabilize the string of drill pipe in a well bore, and a layer of the hardfacing alloy of claim 57 welded to the outer surfaces of the stabilizer ribs subject to the abrasion.

### Claim 60 (depends on 57)

A tool joint for connecting together drill pipe, the tool joint having a cylindrical body, an internally threaded box which has an outer cylindrical surface of a diameter greater than the drill pipe, and an externally threaded pin including, at least one layer of the hardfacing alloy of claim 57 welded to the outer cylindrical surface of one or both of the box or pin, thereby providing surface resistance to abrasion by silicious materials.

### Claim 61 (depends on 60)

The tool joint of claim 60 where, the outer cylindrical surface of one or both the box or pin has a reduced diameter portion extending along a substantial portion of its length, and the layer of hardfacing alloy is welded to the reduced diameter portion of one or both of the box and the pin.

### Claim 62 (depends on 57)

A method of prolonging the life of an industrial product subject to abrasion of the order of silicious materials comprising, welding a layer of the hardfacing alloy of claim 57 to one or more surfaces of the industrial product subject to the abrasion.