# US 2013/0092876 A1 · Silicate luminescent materials and preparation methods thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2013/0092876 A1
- Document ID: US20130092876A1
- Status: Published application
- Kind: A1
- Application number: 13/806,375
- Filed: 2010-08-13
- Published: 2013-04-18
- Earliest claimed: 2010-08-13
- Assignees: Ocean's King Lighting Science & Technology Co., Ltd.
- Inventors: Mingjie Zhou; Wenbo Ma; Qiurong Liao
- Web page: https://patentgrep.com/patent/US20130092876A1

## CPC

- C09K 11/77742: {Silicates}
- C09K 11/025: {non-luminescent particle coatings or suspension media}
- C09K 11/87: containing platina group metals
- B82Y 30/00: Nanotechnology for materials or surface science, e.g. nanocomposites
- Y10S 977/773: Nanoparticle, i.e. structure having three dimensions of 100 nm or less
- C09K: MATERIALS FOR MISCELLANEOUS APPLICATIONS, NOT PROVIDED FOR ELSEWHERE
- B82Y: SPECIFIC USES OR APPLICATIONS OF NANOSTRUCTURES; MEASUREMENT OR ANALYSIS OF NANOSTRUCTURES; MANUFACTURE OR TREATMENT OF NANOSTRUCTURES
- Y10S: TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS

## Abstract

Silicate luminescent materials and preparation methods thereof are provided. The luminescent materials are represented by the general formula: M2aM3bSicO[a+3(b+x)/2+2c]:xCe3+, yM0, M2 is at least one selected from Ca, Sr, Ba, Mg and at least contains Ca, M3 is Sc, Sc and Y, M0 is one selected from metal nano particles of Ag, Au, Pt, Pd or Cu, wherein 2.8≦a≦3.2, 1.8≦b≦2.1, 2.9≦c≦3.3, 0.01≦x≦0.2 and 1×10−4≦y≦1×10−2. Compared to the luminescent materials in the prior art, the said luminescent materials have higher luminous efficiency and more stable performance and structure. The said methods have simple technique and low cost, therefore are appropriate to be used in industry.

## Claims

### Claim 1

A silicate fluorescent powder, having a chemical formula of: M2aM3bSicO[a+3(b+x)/2+2c]:xCe3+, yM0 , wherein 2.8≦a≦3.2, 1.8≦≦b≦2.1, 2.9≦c≦3.3, 0.01≦x≦0.2, 1×10−4≦y≦1×10−2, M2 is a combination of at least one of Sr, Ba and Mg with Ca; M3 is Sc or a combination of Sc with Y; M0 represents a metal nanoparticle selected from one of Ag, Au, Pt, Pd and Cu nanoparticles.

### Claim 2

A method for preparing a silicate fluorescent powder, comprising the steps of:
providing a M0 metal nanoparticle sol;
providing a source compound of M2, a source compound of M3, a source compound of Si, a source compound of Ce and the M0 metal nanoparticle sol according to stoichiometric ratio of corresponding elements in a chemical formula of M2aM3bSicO[a+3(b+x)/2+2c]:xCe3+, yM0 , wherein 2.8≦a≦3.2, 1.8≦b≦2.1, 2.9≦c≦3.3, 0.01≦x≦0.2, 1×10−4≦y≦1×1031 2, M2 is a combination of at least one of Sr, Ba and Mg with Ca; M3 is Sc or a combination of Sc with Y; M0 represents a metal nanoparticle selected from one of Ag, Au, Pt, Pd and Cu nanoparticles;
adding the M0 metal nanoparticle sol and the source compound of M2, a source compound of M3 and a source compound of Ce to an alcoholic solution of the source compound of Si to give a mixed solution;
adjusting the pH of the mixed solution to be acidic, heating in a water bath to conduct reaction, and drying to give a precursor;
pre-calcinating the precursor; and
calcinating the pre-calcinated precursor in a reductive atmosphere to give the silicate fluorescent powder.

### Claim 3 (depends on 2)

The method for preparing a silicate fluorescent powder according to claim 2, wherein:
the source compound of Si is tetraethyl orthosilicate;
the source compound of M2 is at least one of nitrate, sulfate and chloride of M2;
the source compound of M3 is at least one of nitrate, sulfate and chloride of M3; and
the source compound of Ce is at least one of nitrate, sulfate and chloride of Ce.

### Claim 4 (depends on 2)

The method for preparing a silicate fluorescent powder according to claim 2, wherein: a process for preparing the M0 metal nanoparticle sol comprises the steps of:
dissolving a source compound of M0, followed by adding an auxiliary and a reductant; after completion of the reaction, treating with a surface treating agent to give the M0 metal nanoparticle sol;
the content of the added auxiliary in the M0 metal nanoparticle sol is 1.5×10−4 g/mL˜2.1×10−3 g/mL;
the molar ratio of the added reductant to the M0 metal ion is 1.2:1˜4.8:1; and
the content of the added surface treating agent in the M0 metal nanoparticle sol is 1.5×10−4 g/mL˜2.1×10−3 g/mL.

### Claim 5 (depends on 4)

The method for preparing a silicate fluorescent powder according to claim 4, wherein: in the process for preparing the M0 metal nanoparticle sol,
the source compound of M0 is at least one of silver nitrate, chloroauric acid, chloroplatinic acid, palladium chloride and cupric nitrate;
the auxiliary is at least one of polyvinylpyrrolidone, sodium citrate, hexadecyl trimethyl ammonium bromide, sodium dodecylsulfate and sodium dodecylsulphonate;
the reductant is at least one of hydrazine hydrate, ascorbic acid and sodium borohydride; and
the surface treating agent is at least one of polyvinylpyrrolidone and 3-aminopropyl trimethyl siloxane.

### Claim 6 (depends on 2)

The method for preparing a silicate fluorescent powder according to claim 2, wherein: in the process for preparing the mixed solution, the alcohol for the alcoholic solution of the source compound of Si is ethanol.

### Claim 7 (depends on 2)

The method for preparing a silicate fluorescent powder according to claim 2, wherein: in the process for preparing the precursor, the pH of the mixed solution is 3˜6; the heating temperature of the water bath is 60-95° C., and the drying temperature is 80˜120° C.

### Claim 8 (depends on 7)

The method for preparing a silicate fluorescent powder according to claim 7, wherein: in the process for preparing the precursor, the pH of the mixed solution is adjusted with nitric acid.

### Claim 9 (depends on 2)

The method for preparing a silicate fluorescent powder according to claim 2, wherein:
the temperature of the pre-calcination is 700˜1000° C., and the time is 3˜5 h; and
the temperature under which the precursor is calcinated in a reductive atmosphere is 1250˜1500° C., and the time is 2˜12 h.

### Claim 10 (depends on 9)

The method for preparing a silicate fluorescent powder according to claim 9, wherein: the reductive atmosphere is one of N2—H2 mixed reductive atmosphere, CO reductive atmosphere and H2 reductive atmosphere.

### Claim 11

A silicate fluorescent powder, having a chemical formula of:
Ca2.9Sc2Si3O12:0.1 Ce3+, 1×10−3 Ag, Ca2Sr0.8Sc1.8Si2.9O11.315:0.01Ce3+, 1×10−4 Au,
Ca1.5Ba0.7Sr1.0Sc1.5Y0.6Si3.3O13.025:0.05Ce3+, 2×10−3 Pt,
Ca2.74Mg0.06Sc2Si3.1O12.3:0.2Ce3+, 1×10−2 Pd,
Ca1.0Sr1.0Mg0.9Sc1.9Si2.95O11.77:0.08Ce3+, 8×10−4 Cu, or
Ca2.88Sc1.94Y0.06Si3O12:0.12Ce3+, 8×10−3 Ag.