# US 2012/0251823 A1 · Tow prepreg and system and method for forming the same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2012/0251823 A1
- Document ID: US20120251823A1
- Status: Published application
- Kind: A1
- Application number: 13/439,581
- Filed: 2012-04-04
- Published: 2012-10-04
- Earliest claimed: 2011-04-04
- Assignees: Newport Adhesives and Composites, Inc.
- Inventors: Freddy Maldonado; Jesus Fernandez-Marquez; Atsushi Nohara; Paul Kyle
- Web page: https://patentgrep.com/patent/US20120251823A1

## CPC

- B29C 43/24: Calendering
- B29B 15/122: {with a matrix in liquid form, e.g. as melt, solution or latex}
- B29C 43/28: incorporating preformed parts or layers, e.g. compression moulding around inserts or for coating articles
- B29C 70/504: {using rollers or pressure bands (for corrugating B29C53/22)}
- Y10T 428/2918: including free carbon or carbide or therewith [not as steel]
- Y10T 428/2967: Synthetic resin or polymer
- Y10T 428/2969: Polyamide, polyimide or polyester
- B29C: SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING (making preforms B29B11/00; making laminated products by combining previously unconnected layers which become one product whose layers will remain together B32B37/00 - B32B41/00)
- B29B: PREPARATION OR PRETREATMENT OF THE MATERIAL TO BE SHAPED; MAKING GRANULES OR PREFORMS; RECOVERY OF PLASTICS OR OTHER CONSTITUENTS OF WASTE MATERIAL CONTAINING PLASTICS
- Y10T: TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION

## Abstract

The invention provides a tow prepreg having improved productivity and performance. In various embodiments, the tow prepreg has 90% or more resin impregnation and a FAW greater than 600 g/m2. A method of making the prepreg by impregnating each continuous reinforcement fiber strand with a thermosetting resin is also disclosed. In various embodiments, the resin is applied to the reinforcement fiber while flattening the fiber between heated rollers positioned in parallel to each other.

## Claims

### Claim 1

A method for manufacturing a resin impregnated fiber, comprising:
applying flowable resin to a gap defined by a surface of each of two or more rollers, wherein the resin is supplied to the gap from a reservoir formed from said two or more rollers; and
passing at least one continuous fiber through the gap thereby contacting the fiber with the flowable resin, wherein at least one of said two or more rollers rotate in the direction of the passing of the fiber, such that during the passing of the fiber through the said fiber is impregnated with said flowable resin.

### Claim 2 (depends on 1)

The method of claim 1, wherein the fiber is a member of a plurality of fibers forming a tow prepreg.

### Claim 3 (depends on 1)

The method of claim 1, wherein the impregnating is performed under conditions sufficient to prevent the resin from catalyzing.

### Claim 4 (depends on 1)

The method of claim 1, wherein the impregnating is performed under conditions sufficient to prevent the impregnated fiber from plasticizing.

### Claim 5 (depends on 1)

The method of claim 1, wherein the viscosity of the flowable resin applied to the fiber is controlled within a range of about 0.5 poise to about 1000 poise at the impregnation process temperature.

### Claim 6 (depends on 1)

The method of claim 1, wherein the resin prior to impregnation has a viscosity controlled between about 100 poise and about 300,000 poise at about 40° Celsius.

### Claim 7 (depends on 1)

The method of claim 1, wherein the two or more rollers cause the resin to at least partially impregnate the fiber.

### Claim 8 (depends on 1)

The method of claim 1, further comprising: after impregnating the fiber, applying heat directly or indirectly to the resin-impregnated fiber to increase impregnation of the resin in the fiber.

### Claim 9 (depends on 1)

The method of claim 1, further comprising, following a member selected from the impregnation, the heating and a combination thereof, cooling the impregnated fiber.

### Claim 10 (depends on 1)

The method of claim 1, further comprising after the cooling, winding the fiber around a bobbin without a release liner.

### Claim 11 (depends on 1)

The method of claim 1, wherein the resulting fiber has a resin impregnation ratio of at least 90%.

### Claim 12 (depends on 1)

The method of claim 1, further comprising passing a plurality of individual continuous reinforcement fibers between the rollers.

### Claim 13 (depends on 1)

The method of claim 1, wherein, prior to the impregnating, the reinforcement fibers are in a tow shape.

### Claim 14 (depends on 12)

The method of claim 12, wherein the tow is formed of loosely-coupled carbon fibers.

### Claim 15 (depends on 1)

The method of claim 1, wherein the resin is applied using two rollers, the ratio of circumferential velocity of the first roller relative to the second roller being between about 0.7 and about 1.2.

### Claim 16 (depends on 1)

The method of claim 1, wherein the resin is applied using two rollers, a ratio of circumferential velocity of the second roller relative to the first roller being between 0 and about 0.5.

### Claim 17 (depends on 1)

The method of claim 1, wherein the thickness of the resin applied to the gap between the rollers is in a range selected from the group consisting of between about 3 mm and about 12 mm, between about 3 mm and about 8 mm, and between about 3 mm and about 4 mm.

### Claim 18 (depends on 1)

The method of claim 1, wherein the fiber, prior to impregnation, has a tensile modulus of 2500 MPa or more.

### Claim 19 (depends on 1)

The method of claim 1, wherein the fiber is a member selected from the group consisting of carbon fiber, graphite fiber, glass fiber, aramid fiber, and combinations of the same.

### Claim 20 (depends on 1)

The method of claim 1, wherein the resin is a member selected from the group consisting of epoxy resin, bt-resin, phenolic resin, bismaleimide resin, bismaleimide triazine resin, isocyanate resin, vinylester resin, and combinations of the same.

### Claim 21 (depends on 1)

A member selected from a fiber and a tow prepreg which is prepared according to the method of claim 1.

### Claim 22

A system for manufacturing a resin impregnated fiber, comprising:
a first roller having a first cylindrical roller surface, and a second roller having a second cylindrical roller surface, wherein the first and second cylindrical roller surfaces define a flowable resin reservoir and further define a gap between said surfaces for receiving at least one continuous fiber therethrough, and through which the flowable resin is capable of flowing,
the two or more rollers are configured to coat the at least one continuous fiber with the flowable resin thereby impregnating the fiber with the resin as the fiber and the resin pass through the gap, the two or more rollers positioned essentially in parallel, and rotating in the direction of travel of the fiber through the gap.

### Claim 23 (depends on 22)

The system according to claim 22, further comprising:
a heater for heating the reinforcement fiber in the vicinity of the two or more rollers, wherein the heater is configured to maintain the resin-impregnated fiber below a predetermined reaction starting temperature.

### Claim 24 (depends on 22)

The system of claim 22, wherein the first roller and the second flatten the at least one fiber while coating the fiber with resin.

### Claim 25 (depends on 22)

The system of claim 22, wherein a at least a portion of the first cylindrical surface and the second cylindrival surface is maintained at a predetermined temperature between about 70 degrees Celsius and about 80 degrees Celsius.

### Claim 26 (depends on 22)

The system of claim 22, further comprising one or more chilling rollers downstream from the first and second roller for reducing the temperature of the coated fiber, the one or more chilling rollers maintained at a predetermined temperature of about 15 degrees Celsius.

### Claim 27 (depends on 22)

The system of claim 22, further comprising:
a conveyer for delivering the reinforcement fiber to the first and second roller;
a dispenser for dispensing the flowable resin to the first and second roller; and
a winder roller for winding up the fiber prior to curing.

### Claim 28 (depends on 22)

A system for forming a resin impregnated fiber, comprising:
the system for forming a tow prepreg of claim 22; and
means for curing the fiber, wherein the system for forming the impregnated fiber and the curing means are distinct.

### Claim 29 (depends on 27)

The system of claim 27, wherein the conveyor conveys the fiber between about 30 feet/minute and about 35 feet/minute.

### Claim 30 (depends on 22)

The system of claim 22, wherein the resulting fiber has a weight per unit area (FAW) of at least 550 grams/m2.

### Claim 31 (depends on 22)

The system of claim 22, wherein the resulting fiber is composed of less than about 35% by weight resin.

### Claim 32

A method of forming a composite film structure comprising:
providing a continuous reinforcement fiber; and
impregnating the fiber with a flowable resin, the impregnating comprising:
laying the flowable adhesive resin on a surface of the fiber;
applying pressure to the resin and the fiber; and
heating the resin and the fiber to a predetermined temperature to cause at least partial impregnation of the fiber with the resin,
wherein the predetermined temperature is below a reaction starting temperature of the resin impregnated in the fiber.

### Claim 33 (depends on 32)

The method according to claim 32, wherein the impregnating is performed under conditions sufficient to cause at least partial impregnation of the fiber by the resin without significantly catalyzing the impregnated resin.

### Claim 34

A tow prepreg comprising:
a tow material formed of a plurality of reinforcement fibers, the reinforcement fibers being a member selected from the group consisting of carbon fiber, graphite fiber, glass fiber, aramid fiber, and combinations of the same; and
a resin impregnated in the tow material, resin being a member selected from the group consisting of epoxy resin, bt-resin, phenolic resin, bismaleimide resin, bismaleimide triazine resin, isocyanate resin, vinylester resin, and combinations of the same;
wherein the prepreg has a fiber weight per unit area (FAW) of more than about 600 grams/m2.

### Claim 35 (depends on 34)

The two prepreg according to claim 34, wherein the impregnation ratio of the fiber with the resin is at least 90%.