# US 2012/0241052 A1 · Ferritic stainless steel and method of manufacturing the same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2012/0241052 A1
- Document ID: US20120241052A1
- Status: Published application
- Kind: A1
- Application number: 13/337,014
- Filed: 2011-12-23
- Published: 2012-09-27
- Earliest claimed: 2011-03-25
- Assignees: Posco
- Inventors: Sang-Seok Kim; Do-leal Yoo; Bo-Sung Seo
- Web page: https://patentgrep.com/patent/US20120241052A1

## CPC

- C22C 38/22: with molybdenum or tungsten
- C21D 6/002: {containing Cr (C21D6/004 takes precedence)}
- C21D 8/0273: {Final recrystallisation annealing}
- C21D 8/0473: {Final recrystallisation annealing}
- C22C 38/001: {containing N}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/26: with niobium or tantalum
- C22C 38/28: with titanium or zirconium
- C21D 2211/005: Ferrite
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)

## Abstract

The present disclosure relates to a ferritic stainless steel and fabrication method of a ferritic stainless steel comprising, by weight %, C: above 0 wt % to 0.01 wt % or less, Si: above 0 wt % to 0.5 wt % or less, Mn: above 0 wt % to 2.0 wt % or less, P: 0 wt % or more to 0.04 wt % or less, S: 0 wt % or more to 0.02 wt % or less, Cr: 12 wt % or more to 19 wt % or less, Mo: 0 wt % or more to 1.0 wt % or less, W: 2 wt % of more to 7 wt % or less, Ti: 0 wt % or more to 0.3 wt % or less, Nb: above 0 wt % to 0.6 wt % or less, N: above 0 wt % to 0.01 wt % or less, Al: 0 wt % or more to 0.1 wt % or less; and the balance of Fe and other inevitable impurities.

## Claims

### Claim 1

A ferritic stainless steel comprising:
by weight %, C: above 0 wt % to 0.01 wt % or less, Si: above 0 wt % to 0.5 wt % or less, Mn: above 0 wt % to 2.0 wt % or less, P: 0 wt % or more to 0.04 wt % or less, S: 0 wt % or more to 0.02 wt % or less, Cr: 12 wt % or more to 19 wt % or less, Mo: 0 wt % or more to 1.0 wt % or less, W: 2 wt % or more to 7 wt % or less, Ti: 0 wt % or more to 0.3 wt % or less, Nb: above 0 wt % to 0.6 wt % or less, N: above 0 wt % to 0.01 wt % or less, Al: 0 wt % or more to 0.1 wt % or less; and the balance of Fe and other inevitable impurities.

### Claim 2 (depends on 1)

The ferritic stainless steel according to claim 1, wherein Mo is 0.8 wt % or less, by weight %.

### Claim 3 (depends on 2)

The ferritic stainless steel according to claim 2, wherein a hot-annealed structure of the ferritic stainless steel comprises a sigma phase of 5% or less.

### Claim 4 (depends on 1)

The ferritic stainless steel according to claim 1, wherein W is 3 wt % or more to 6 wt % or less, by weight %.

### Claim 5 (depends on 1)

The ferritic stainless steel according to claim 1, wherein Mo wt %+0.83W wt % is 3.5 wt % or more to 5 wt % or less, by weight %.

### Claim 6 (depends on 1)

The ferritic stainless steel according to claim 1, wherein [(Ti wt %+1/2Nb wt %)/(C wt %+N wt %)] is 19.5 or more to 32 or less.

### Claim 7 (depends on 1)

The ferritic stainless steel according to claim 1, wherein ductile-brittleness transition temperature (DBTT) is 90° C. or less.

### Claim 8 (depends on 1)

The ferritic stainless steel according to claim 1, wherein the ferritic stainless steel satisfies the following equation: −184.6+3.2(Cr wt %)+27.5(Mo wt %)+4243.4(C wt %+N wt %)−295.6(Al wt %)+0.9[Nb wt %/(C wt %+N wt %)] 90.

### Claim 9

A fabrication method of a ferritic stainless steel comprising, by weight %, C: above 0 wt % to 0.01 wt % or less, Si: above 0 wt % to 0.5 wt % or less, Mn: above 0 wt % to 2.0 wt % or less, P: 0 wt % or more to 0.04 wt % or less, S: 0 wt % or more to 0.02 wt % or less, Cr: 12 wt % or more to 19 wt % or less, Mo: 0 wt % or more to 1.0 wt % or less, W: 2 wt % or more to 7 wt % or less, Ti: 0 wt % or more to 0.3 wt % or less, Nb: above 0 wt % to 0.6 wt % or less, N: above 0 wt % to 0.01 wt % or less, Al: 0 wt % or more to 0.01 wt % or less; and the balance of Fe and other inevitable impurities,
wherein
the fabrication method of the ferritic stainless steel sheet comprises:
providing a slab;
heating the slab;
hot annealing;
cold annealing; and
cold rolling.

### Claim 10 (depends on 9)

The fabrication method of a ferritic stainless steel according to claim 9, wherein Mo is 0.8 wt % or less, by weight %.

### Claim 11 (depends on 9)

The fabrication method of a ferritic stainless steel according to claim 9, wherein W is 3 wt % or more to 6 wt % or less, by weight %.

### Claim 12 (depends on 9)

The fabrication method of a ferritic stainless steel according to claim 9, wherein:
Mo wt %+0.83W wt % is 3.5 wt % or more to 5 wt % or less, by weight %.

### Claim 13 (depends on 9)

The fabrication method of a ferritic stainless steel according to claim 9, wherein:
[(Ti wt %+1/2Nb wt %)/(C wt %+N wt %)] is 19.5 or more to 32 or less.

### Claim 14 (depends on 9)

The fabrication method of a ferritic stainless steel according to claim 9, wherein:
ductile-brittleness transition temperature (DBTT) is 90° C. or less.

### Claim 15 (depends on 9)

The fabrication method of a ferritic stainless steel according to claim 9, wherein the ferritic stainless steel satisfies the following equation:
−184.6+3.2(Cr wt %)+27.5(Mo wt %)+4243.4(C wt %+N wt %)−295.6(Al wt %)+0.9[Nb wt %/(C wt %+N wt %)]<90.

### Claim 16 (depends on 9)

The fabrication method of a ferritic stainless steel according to claim 9, wherein grain size is ASTM No. 3 or more.

### Claim 17 (depends on 9)

The fabrication method of a ferritic stainless steel according to claim 9, wherein heating the slab has slab heating temperature that is 1180° C. or more to 1240° C. or less, with respect to slab temperature.

### Claim 18 (depends on 9)

The fabrication method of a ferritic stainless steel according to claim 9, wherein hot annealing has a hot-annealing temperature that is 1020° C. or more to 1070° C. or less, with respect to strip temperature.

### Claim 19 (depends on 9)

The fabrication method of a ferritic stainless steel according to claim 9, wherein cold annealing has a cold-annealing temperature that is 1030° C. or more to 1080° C. or less, with respect to strip temperature.

### Claim 20 (depends on 9)

The fabrication method of a ferritic stainless steel according to claim 9, wherein (cold-annealing temperature)/(hot-annealing temperature) is 1.0 or more to 1.1 or less, and wherein the cold-annealing temperature is the temperature in cold-annealing and the hot-annealing temperature is the temperature in hot annealing.