# US 2010/0168336 A1 · Process for the manufacture of polybutylene terephthalate copolymers from polyethylene terephthalate, and compositions and articles thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2010/0168336 A1
- Document ID: US20100168336A1
- Status: Published application
- Kind: A1
- Application number: 12/346,108
- Filed: 2008-12-30
- Published: 2010-07-01
- Earliest claimed: 2008-12-30
- Assignees: Sabic Innovative Plastics IP B.V.
- Inventors: Kristen Cohoon-Brister
- Web page: https://patentgrep.com/patent/US20100168336A1

## CPC

- C08G 63/916: {Dicarboxylic acids and dihydroxy compounds}
- C08J 11/24: containing hydroxyl groups
- C08L 67/02: Polyesters derived from dicarboxylic acids and dihydroxy compounds (C08L67/06 takes precedence)
- C08J 2367/02: Polyesters derived from dicarboxylic acids and dihydroxy compounds; (C08J2367/06 takes precedence)
- C08L 27/06: Homopolymers or copolymers of vinyl chloride
- C08L 27/08: Homopolymers or copolymers of vinylidene chloride
- C08L 67/04: Polyesters derived from hydroxycarboxylic acids, e.g. lactones (C08L67/06 takes precedence)
- C08L 77/02: Polyamides derived from omega-amino carboxylic acids or from lactams thereof (C08L77/10 takes precedence)
- Y02W 30/62: Plastics recycling; Rubber recycling
- C08G: MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
- C08J: WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H (working, e.g. shaping, of plastics B29)
- C08L: COMPOSITIONS OF MACROMOLECULAR COMPOUNDS (compositions based on polymerisable monomers C08F, C08G; artificial filaments or fibres D01F; textile treating compositions D06)
- Y02W: CLIMATE CHANGE MITIGATION TECHNOLOGIES RELATED TO WASTEWATER TREATMENT OR WASTE MANAGEMENT

## Abstract

A process comprises depolymerizing, with 1,4-butane diol, a first polymer comprising a polyethylene terephthalate component in the presence of at least one second polymer selected from the group consisting of polyvinyl chlorides, polyvinylidene chlorides, polyamides, polylactic acid, and combinations thereof to produce a molten mixture; and polymerizing the molten mixture under conditions sufficient to form a modified polybutylene terephthalate copolymer. The modified PBT comprises (a) at least one polyethylene terephthalate component residue, and (b) a member selected from the group consisting of (i) the at least one second polymer selected from the group consisting of polyvinyl chlorides, polyvinylidene chlorides, polyamides, polylactic acid, and combinations thereof; (ii) the at least one residue derived from the second polymer; and (iii) combinations thereof.

## Claims

### Claim 1

A process comprising:
depolymerizing, with 1,4-butane diol,
a first polymer comprising a polyethylene terephthalate component selected from the group consisting of polyethylene terephthalate homopolymers, polyethylene terephthalate copolymers, and combinations thereof, in the presence of
at least one second polymer selected from the group consisting of polyvinyl chlorides, polyvinylidene chlorides, polyamides, polylactic acid, and combinations thereof,
in a reactor at a first temperature and a first pressure that is at least atmospheric pressure, for a time and under conditions effective to produce a molten mixture comprising
a first component selected from the group consisting of oligomers containing ethylene terephthalate groups, oligomers containing ethylene isophthalate groups, oligomers containing diethylene terephthalate groups, oligomers containing diethylene isophthalate groups, oligomers containing butylene terephthalate groups, oligomers containing butylene isophthalate groups, covalently bonded oligomeric moieties containing at least two of the foregoing groups, 1,4-butane diol, ethylene glycol, and combinations thereof; and
a second component selected from the group consisting of
(i) the at least one second polymer selected from the group consisting of polyvinyl chlorides, polyvinylidene chlorides, polyamides, polylactic acid, and combinations thereof;
(ii) at least one residue derived from the at least one second polymer selected from the group consisting of polyvinyl chlorides, polyvinylidene chlorides, polyamides, polylactic acid, and combinations thereof; and
(iii) combinations thereof; and
polymerizing the molten mixture at a second temperature that is higher than the first temperature, a second pressure that is lower than the first pressure and that is subatmospheric pressure, with agitation and under an inert atmosphere, for a time and under conditions sufficient to form a modified polybutylene terephthalate copolymer comprising
(a) at least one polyethylene terephthalate component residue, and
(b) a member selected from the group consisting of
(i) the at least one second polymer selected from the group consisting of polyvinyl chlorides, polyvinylidene chlorides, polyamides, polylactic acid, and combinations thereof;
(ii) the at least one residue derived from the second polymer; and
(iii) combinations thereof.

### Claim 2 (depends on 1)

The process of claim 1, wherein depolymerizing is conducted with agitation under an inert atmosphere.

### Claim 3 (depends on 1)

The process of claim 1, wherein the at least one polyethylene terephthalate component residue is selected from the group consisting of ethylene glycol groups, diethylene glycol groups, isophthalic acid groups, antimony-containing compounds, germanium-containing compounds, titanium-containing compounds, cobalt-containing compounds, tin containing compounds, aluminum, aluminum salts, 1,3-cyclohexane dimethanol isomers, 1,4-cyclohexane dimethanol isomers, alkali salts, alkaline earth metal salts, phosphorus-containing compounds and anions, sulfur-containing compounds and anions, naphthalene dicarboxylic acids, 1,3-propanediol groups, and combinations thereof.

### Claim 4 (depends on 1)

The process of claim 1, wherein the at least one polyethylene terephthalate component residue is selected from the group consisting of ethylene glycol, diethylene glycol, isophthalic acid, cobalt-containing compounds, antimony-containing compounds, isophthalic acid groups, and combinations thereof.

### Claim 5 (depends on 1)

The process of claim 1, wherein the at least one polyethylene terephthalate component residue is selected from the group consisting of cis isomer of 1,3-cyclohexane dimethanol, cis isomer of 1,4-cyclohexane dimethanol, the trans isomer of 1,3-cyclohexane dimethanol, trans isomer of 1,4-cyclohexane dimethanol and combinations thereof.

### Claim 6 (depends on 1)

The process of claim 1, wherein the at least one polyethylene terephthalate component residue is selected from the group consisting of ethylene glycol groups, diethylene glycol groups, and cyclohexane dimethanol groups; and the polyethylene terephthalate component residue is in an amount ranging from 0.1 to 10 mole %, based on 100 mole % of glycol in the modified polybutylene terephthalate copolymer.

### Claim 7 (depends on 6)

The process of claim 6, wherein the at least one polyethylene terephthalate component residue further comprises isophthalic acid groups in an amount ranging from more than 0 to 10 mole %, based on 100 mole % of acid functionality in the modified polybutylene terephthalate random copolymer.

### Claim 8 (depends on 1)

The process of claim 1, wherein the modified polybutylene terephthalate copolymer has a melting temperature of more than 200° C. and an intrinsic viscosity ranging from 0.5 to 1.4 dL/g, and comprising

### Claim 9 (depends on 1)

The process of claim 1, wherein
prior to depolymerizing the polyethylene terephthalate component, the second polymer comprises more than 0 to less than 290 ppm of polyvinyl chloride, based on the total parts by weight of the polyethylene terephthalate component; and
a sample molded from the modified polybutylene terephthalate copolymer has an unnotched Izod strength of 1500 to 2500 J/m, measured in accordance with ASTM D256, and a tensile elongation at break of at least 100%, measured in accordance with ASTM D638.

### Claim 10 (depends on 1)

The process of claim 1, wherein
prior to depolymerizing the polyethylene terephthalate component, the second polymer comprises more than 0 to less than 5.7 wt. % of a polyamide as the second polymer, based on the total weight of the polyethylene terephthalate component, wherein the polyamide is Nylon 6; and
a molded sample of the modified polybutylene terephthalate copolymer has a tensile elongation at break of at least 100%, measured in accordance with ASTM D638.

### Claim 11 (depends on 1)

The process of claim 1, wherein
prior to depolymerizing the polyethylene terephthalate component, the second polymer comprises more than 0 to less than 1.45 wt. % of a polyamide as the second polymer, based on the total weight of the polyethylene terephthalate component;
the polyamide is Nylon 6; and
a molded sample of the modified polybutylene terephthalate copolymer has a heat deflection temperature at 0.455 MPa of at least 90° C., measured in accordance with ASTM D648.

### Claim 12 (depends on 1)

The process of claim 1, wherein
prior to depolymerizing the polyethylene terephthalate component, the second polymer comprises more than 0 to less than 5.7 wt. % of a polyamide as the second polymer, based on the total weight of the polyethylene terephthalate component;
the polyamide is Nylon 6,6; and
a molded sample of the modified polybutylene terephthalate copolymer has a tensile elongation at break that is at least 100%, measured in accordance with ASTM D638.

### Claim 13 (depends on 1)

The process of claim 1, wherein
prior to depolymerizing the polyethylene terephthalate component, the second polymer comprises more than 0 to less than 4.6 wt. % of a polyamide as the second polymer, based on the total weight of the polyethylene terephthalate component;
the polyamide is Nylon 6,6; and
a molded sample of the modified polybutylene terephthalate copolymer has a heat deflection temperature at 0.455 MPa that is at least 70° C., measured in accordance with ASTM D648.

### Claim 14 (depends on 1)

The process of claim 1, wherein depolymerizing the polyethylene terephthalate is carried out at a temperature from 180° C. to 230° C.

### Claim 15 (depends on 1)

The process of claim 1, wherein depolymerizing the polyethylene terephthalate component is carried out at a pressure from 100 kPa to 500 kPa absolute.

### Claim 16 (depends on 1)

The process of claim 1, wherein depolymerizing the polyethylene terephthalate component is carried out for at least 30 minutes.

### Claim 17 (depends on 1)

The process of claim 1, wherein the second temperature is from 230° C. to 260° C.

### Claim 18 (depends on 1)

The process of claim 1, wherein the second pressure is less than 0.3 kPa absolute.

### Claim 19 (depends on 1)

The process of claim 1, wherein the polymerization of the molten mixture is carried out for at least 60 minutes.

### Claim 20 (depends on 1)

The process of claim 1, wherein a catalyst is present during a step selected from the group consisting of (i) depolymerizing the polyethylene terephthalate component, (ii) polymerization of the molten mixture, and (iii) combinations thereof.

### Claim 21 (depends on 1)

The process of claim 1, wherein a basic compound is present during a step selected from the group consisting of (i) depolymerizing the polyethylene terephthalate component, (ii) polymerization of the molten mixture, and (iii) a combination thereof.

### Claim 22 (depends on 1)

The process of claim 1, wherein the process is carried out in at least two reactors.

### Claim 23

A composition comprising a modified polybutylene terephthalate copolymer having a melting temperature of more than 200° C. and an intrinsic viscosity ranging from 0.5 to 1.4 dL/g, and comprising
(a) at least one residue derived from a polyethylene terephthalate component; and
(b) a member selected from the group consisting of
(i) at least one polymer selected from the group consisting of polyvinyl chlorides, polyvinylidene chlorides, polyamides, polylactic acid, and combinations thereof;
(ii) at least one residue derived from a polymer selected from the group consisting of polyvinyl chlorides, polyvinylidene chlorides, polyamides, polylactic acid, and combinations thereof; and
(iii) combinations thereof.

### Claim 24 (depends on 23)

The composition of claim 23, wherein
the at least one polymer comprises polyvinyl chloride as the second polymer, present in an amount of more than 0 and less than 220 ppm of, based on the total parts by weight of the polyethylene terephthalate component; and
a molded sample of the composition has an unnotched Izod strength of 1500 to 2500 J/m, measured in accordance with ASTM D256, and a tensile elongation at break that is at least 100%, measured in accordance with ASTM D638.

### Claim 25 (depends on 23)

The composition of claim 23, wherein
the at least one polymer comprises Nylon 6 as the second polymer, present in an amount of more than 0 and less than 5.7 wt. % of, based on the total weight of the polyethylene terephthalate component, and
a molded sample of the composition has a tensile elongation at break that is at least 100%, measured in accordance with ASTM D638.

### Claim 26 (depends on 23)

The composition of claim 23, wherein
the at least one polymer comprises Nylon 6 as the second polymer, present in an amount of more than 0 and less than 1.45 wt. %, based on the total weight of the polyethylene terephthalate component; and
a molded sample of the modified polybutylene terephthalate copolymer has a heat deflection temperature at 0.455 MPa that is at least 90° C., measured in accordance with ASTM D648.

### Claim 27 (depends on 23)

The composition of claim 23, wherein
the at least one polymer comprises Nylon 6,6 as the second polymer, present in an amount of more than 0 and less than 5.7 wt. %, based on the total weight of the polyethylene terephthalate component; and
a molded sample of the modified polybutylene terephthalate copolymer has a tensile elongation at break that is at least 100%, measured in accordance with ASTM D638.

### Claim 28 (depends on 23)

The composition of claim 23, wherein
the at least one polymer comprises Nylon 6,6 as the second polymer, present more than 0 and less than 4.6 wt. %, based on the total weight of the polyethylene terephthalate component, and
a molded sample of the modified polybutylene terephthalate copolymer has a heat deflection temperature at 0.455 MPa that is at least 70° C., measured in accordance with ASTM D648.

### Claim 29 (depends on 23)

The composition of claim 23, wherein the residue derived from the polyethylene terephthalate component is selected from the group consisting of ethylene glycol groups, diethylene glycol groups, isophthalic acid groups, antimony-containing compounds, germanium-containing compounds, titanium-containing compounds, cobalt-containing compounds, tin containing compounds, aluminum, aluminum salts, 1,3-cyclohexane dimethanol isomers, 1,4-cyclohexane dimethanol isomers, alkali salts, alkaline earth metal salts, phosphorus-containing compounds and anions, sulfur-containing compounds and anions, napthalene dicarboxylic acids, 1,3-propanediol groups, and combinations thereof.

### Claim 30 (depends on 23)

The composition of claim 23, wherein the at least one residue derived from the polyethylene terephthalate component comprises mixtures of ethylene glycol and diethylene glycol.

### Claim 31 (depends on 23)

An article comprising the composition of claim 23.

### Claim 32

A composition comprising a modified polybutylene terephthalate copolymer having a melting temperature of more than 200° C. and an intrinsic viscosity ranging from 0.5 to 1.4 dL/g, and comprising
(a) at least one residue derived from a polyethylene terephthalate component; and
(b) a member selected from the group consisting of
(i) at least one polymer selected from the group consisting of polyvinyl chlorides, polyvinylidene chlorides, polyamides, polylactic acid, and combinations thereof;
(ii) at least one residue derived from a polymer selected from the group consisting of polyvinyl chlorides, polyvinylidene chlorides, polyamides, polylactic acid; and combinations thereof; and
(iii) combinations thereof;
wherein
the modified polybutylene terephthalate copolymer is derived from a polyethylene terephthalate mixture comprising a second polymer selected from the group consisting of
more than 0 to less than 290 ppm polyvinyl chloride,
more than 0 to less than 5.7 wt % Nylon 6;
more than 0 to less than 5.7 wt % Nylon 6,6; and
optionally, more than 0 to less than 8 wt % polylactic acid, each based on the parts by weight or weight of the polyethylene terephthalate component; and
the residue derived from the polyethylene terephthalate component is selected from the group consisting of ethylene glycol groups, diethylene glycol groups, isophthalic acid groups, antimony-containing compounds, germanium-containing compounds, titanium-containing compounds, cobalt-containing compounds, tin containing compounds, aluminum, aluminum salts, 1,3-cyclohexane dimethanol isomers, 1,4-cyclohexane dimethanol isomers, alkali salts, alkaline earth metal salts, phosphorus-containing compounds and anions, sulfur-containing compounds and anions, napthalene dicarboxylic acids, 1,3-propanediol groups, and combinations thereof.

### Claim 33 (depends on 32)

The composition of claim 32, wherein the at least one residue derived from the polyethylene terephthalate component comprises mixtures of ethylene glycol and diethylene glycol.

### Claim 34 (depends on 32)

An article comprising the composition of claim 32.