# US 2010/0167087 A1 · Method of providing a metallic coating layer and substrate provided with said coating layer

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2010/0167087 A1
- Document ID: US20100167087A1
- Status: Published application
- Kind: A1
- Application number: 12/667,286
- Filed: 2008-07-11
- Published: 2010-07-01
- Earliest claimed: 2007-07-13
- Assignees: Hille & MüLler GmbH
- Inventors: Jacques Hubert Olga Joseph Wijenberg; Daniël Adriaan De Vreugd; Ilja Portegies Zwart
- Web page: https://patentgrep.com/patent/US20100167087A1

## CPC

- C25D 3/562: {containing more than 50% by weight of iron or nickel or cobalt}
- C25D 5/14: two or more layers being of nickel or chromium, e.g. duplex or triplex layers
- C25D 5/48: After-treatment of electroplated surfaces
- C25D 7/00: Electroplating characterised by the article coated
- Y10T 428/12944: Ni-base component
- C25D: PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR
- Y10T: TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION

## Abstract

This invention relates to a method for producing a metallic coating layer comprising nickel and molybdenum on an electrically conductive substrate by electrodeposition from an aqueous solution including nickel salts, gluconate anions and citrate anions wherein the substrate acts as the cathode and wherein molybdate is added and wherein the pH of the aqueous solution is adjusted between 5.0 and 8.5. The invention also relates to an electrically conductive substrate provided with such a metallic coating layer electrodeposited from the aqueous solution.

## Claims

### Claim 1

A method for producing a metallic coating layer comprising nickel and molybdenum on an electrically conductive substrate by electrodeposition from an aqueous solution comprising nickel salts, gluconate anions and citrate anions wherein the substrate acts as the cathode and wherein molybdate is added and wherein the pH of the aqueous solution is adjusted between 5.0 and 8.5.

### Claim 2 (depends on 1)

The method according to claim 1, wherein a stress reliever is added for relieving or preventing internal stresses in the coating layer.

### Claim 3 (depends on 1)

The method according to claim 1, wherein the gluconate and citrate are added to the solution as sodium gluconate and sodium citrate.

### Claim 4 (depends on 1)

The method according to claim 1, wherein the nickel salt is nickel sulphate and/or nickel chloride.

### Claim 5 (depends on 1)

The method according to claim 1, wherein the aqueous solution comprises a molybdate, at a concentration of 0.008 mol/l to 0.10 mol/l.

### Claim 6 (depends on 1)

The method according to claim 1, wherein the aqueous solution comprises between 0.005 and 0.5 mol/l sodium gluconate.

### Claim 7 (depends on 1)

The method according to claim 1, wherein the aqueous solution is maintained at a temperature between 30 and 80° C.

### Claim 8 (depends on 1)

The method according to claim 1, wherein the cathodic current density is chosen such that the current efficiency is at least 30%.

### Claim 9 (depends on 1)

The method according to claim 1, wherein the cathodic current density is at least 8.5 A/dm2.

### Claim 10 (depends on 1)

The method according to claim 1, wherein the cathodic current density is at least 12.5 A/dm2.

### Claim 11 (depends on 1)

The method according to claim 1, wherein the mass transfer rate is enhanced by eductors or rotating objects.

### Claim 12 (depends on 1)

The method according to claim 1, wherein the metallic coating layer comprising nickel and molybdenum is coated by a metallic chromium layer and wherein the coating system comprising the metallic coating and the chromium layer are subjected to a diffusion annealing step to form a metallic coating layer comprising a Ni—Mo—Cr alloy layer.

### Claim 13 (depends on 12)

The method according to claim 12, wherein the metallic coating layer consists substantially of said Ni—Mo—Cr alloy.

### Claim 14 (depends on 1)

The method according to claim 1, wherein the aqueous solution comprises
0.53 to 1.06 mol/l NiSO4
0.028 to 0.68 mol/l NiCl2
0.008 to 0.08 mol/l alkali metal molybdate
0.45 to 0.54 mol/l sodium citrate
0.023 to 0.207 mol/l sodium gluconate
0.055 to 1.33 mol/l ammonium from a suitable ammonium salt such as ammonium sulphate.

### Claim 15 (depends on 1)

The method according to claim 1, wherein the aqueous solution comprises
concentration
compound
Formula
g/l
M (or mol/l)
Nickel sulphate
NiSO4 (× 6 H2O)
142
0.540
Nickel chloride
NiCl2 (× 6 H2O)
30
0.126
Sodium molybdate
Na2MoO4 (× 2 H2O)
12.1
0.050
Ammonium sulphate
(NH4)2SO4
34
0.257
Sodium citrate
Na3C6H5O7 (× 2 H2O)
140
0.476
Sodium gluconate
Na2C12H22O14
30
0.138
and wherein the pH is maintained at 6.1±0.2.

### Claim 16 (depends on 1)

Electrically conductive substrate provided with a metallic coating layer comprising nickel and molybdenum provided by electrodepositing said coating layer from an aqueous solution according to claim 1.

### Claim 17 (depends on 16)

Substrate according to claim 16, wherein the metallic coating layer comprising nickel and molybdenum comprises at least 5% in wt of Mo and/or at most 30% in wt of Mo.

### Claim 18 (depends on 16)

Substrate according to claim 16, wherein the metallic coating layer comprising nickel and molybdenum comprises between 10% in wt of Mo and 20% in wt of Mo.

### Claim 19 (depends on 16)

Substrate according to claim 16 wherein the metallic coating layer comprising nickel and molybdenum comprises at least 10% of Mo.

### Claim 20 (depends on 16)

Substrate according to claim 16, wherein the metallic coating layer comprising nickel and molybdenum is provided with a metallic chromium layer.

### Claim 21 (depends on 16)

Substrate according to claim 16, wherein the chromium from the metallic chromium layer has at least partly diffused into the metallic coating layer comprising nickel and molybdenum thereby forming a Ni—Mo—Cr alloy layer.

### Claim 22 (depends on 1)

The method according to claim 1, wherein a stress reliever is added, wherein the stress reliever is ammonium sulphate or ammonium molybdate.

### Claim 23 (depends on 14)

The method according to claim 14, wherein the pH is maintained between 5.75 and 7.25.