# US 2010/0143184 A1 · Method for manufacturing metal nanorods and use thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2010/0143184 A1
- Document ID: US20100143184A1
- Status: Published application
- Kind: A1
- Application number: 12/704,364
- Filed: 2010-02-11
- Published: 2010-06-10
- Earliest claimed: 2003-05-13
- Assignees: Yasuro Niidome; Mitsubishi Materials Corporation; Dai Nippon Toryo Co., Ltd.
- Inventors: Yasuro Niidome; Sunao Yamada; Koji Nishioka; Hideya Kawasaki; Hiroki Hirata; Daigou Mizoguchi; Yoshiaki Takata; Jun-etsu Satoh; Masaoki Ishihara; Masanori Nagai; Masato Murouchi
- Web page: https://patentgrep.com/patent/US20100143184A1

## CPC

- B22F 9/24: starting from liquid metal compounds, e.g. solutions
- B22F 1/0547: {Nanofibres or nanotubes}
- B82Y 30/00: Nanotechnology for materials or surface science, e.g. nanocomposites
- C30B 7/00: Single-crystal growth from solutions using solvents which are liquid at normal temperature, e.g. aqueous solutions (from molten solvents C30B9/00; by normal or gradient freezing C30B11/00; under a protective fluid C30B27/00)
- C30B 7/14: the crystallising materials being formed by chemical reactions in the solution
- C30B 29/605: {Products containing multiple oriented crystallites, e.g. columnar crystallites}
- B22F 2999/00: Aspects linked to processes or compositions used in powder metallurgy
- Y10S 977/762: Nanowire or quantum wire, i.e. axially elongated structure having two dimensions of 100 nm or less
- Y10S 977/896: Chemical synthesis, e.g. chemical bonding or breaking
- B22F: WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER (making alloys by powder metallurgy C22C); APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B82Y: SPECIFIC USES OR APPLICATIONS OF NANOSTRUCTURES; MEASUREMENT OR ANALYSIS OF NANOSTRUCTURES; MANUFACTURE OR TREATMENT OF NANOSTRUCTURES
- C30B: SINGLE-CRYSTAL GROWTH (by using ultra-high pressure, e.g. for the formation of diamonds, B01J3/06); UNIDIRECTIONAL SOLIDIFICATION OF EUTECTIC MATERIAL OR UNIDIRECTIONAL DEMIXING OF EUTECTOID MATERIAL; REFINING BY ZONE-MELTING OF MATERIAL (zone-refining of metals or alloys C22B); PRODUCTION OF A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE (casting of metals, casting of other substances by the same processes or devices B22D; working of plastics B29; modifying the physical structure of metals or alloys C21D, C22F); SINGLE CRYSTALS OR HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE; AFTER-TREATMENT OF SINGLE CRYSTALS OR A HOMOGENEOUS POLYCRYSTALLINE MATERIAL WITH DEFINED STRUCTURE (for producing semiconductor devices or parts thereof H10); APPARATUS THEREFOR
- Y10S: TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS

## Abstract

A method for manufacturing metal nanorods includes: a step of adding a reducing agent to a metallic salt solution; a step of radiating light into the metallic salt solution containing the reducing agent; and a step of leaving the light-radiated metallic salt solution containing the reducing agent stationary in a dark place so as to grow metal nanorods. Metal nanorods can be also grown by forming a mixed solution by fractionating the above light-radiated metallic salt solution and mixing the fractionated metallic salt solution into a non-radiated metallic salt solution containing the reducing agent, or mixing a non-radiated metallic salt solution and the reducing agent into the above light-radiated metallic salt solution; and leaving the mixed solution stationary in a dark place so as to grow metal nanorods.

## Claims

### Claim at position 1

1-2. (canceled)

### Claim 3

A method for manufacturing metal nanorods, the method comprising:
a step of chemically reducing a metallic salt solution;
a step of radiating ultraviolet light into the chemically reduced solution for a period of 5 to 15 minutes so as to generate seed metal nano-particles in the shape of a rod;
a step of fractionating the ultraviolet light-radiated metallic salt solution and mixing the fractionated metallic salt solution with a non-radiated metallic salt solution containing the reducing agent; and
a step of growing metal nanorods from the seed metal nano-particles, by leaving the mixed seed solution containing the reducing agent stationary for a period of 30 to 60 minutes in a place where the ultraviolet light is turned off.

### Claim 4

A method for manufacturing gold nanorods, the method comprising:
a step of chemically reducing an auric salt solution;
a step of radiating ultraviolet light into the chemically reduced solution for a period of 5 to 15 minutes so as to generate seed gold nano-particles in the shape of a rod; and
a step of mixing a non-radiated auric salt solution containing the reducing agent into the light-radiated auric salt solution; and
a step of growing gold nanorods from the seed gold nano-particles, by leaving the mixed seed solution containing the reducing agent stationary for a period of 30 to 60 minutes in a place where the ultraviolet light is turned off.

### Claim 5

(canceled)

### Claim 6 (depends on 3)

The method for manufacturing gold nanorods according to claim 3, wherein ultraviolet light is radiated into a auric salt solution containing a surfactant along with the reducing agent; a small quantity of the light-radiated solution is fractionated to use as a seed solution; and the seed solution is mixed into a non-radiated auric salt solution containing the reducing agent in which a high concentration of the surfactant is added and gold nanorods are grown from the seed gold nano-particles, by leaving the mixed seed solution containing the reducing agent stationary for a period of 30 to 60 minutes in a place where the ultraviolet light is turned off.

### Claim 7 (depends on 4)

The method for manufacturing gold nanorods according to claim 4, wherein a auric salt solution containing a surfactant along with the reducing agent is used; ultraviolet light is radiated into the auric salt solution for forming a seed gold nano-particles, a non-radiated auric salt solution not containing a surfactant and the reducing agent are mixed into the light-radiated auric salt solution; and gold nanorods are grown from the seed gold nano-particles, by leaving the mixed seed solution containing the reducing agent stationary for a period of 30 to 60 minutes in a place where the ultraviolet light is turned off.

### Claim at position 7

8-9. (canceled)

### Claim 10 (depends on 6)

The method for manufacturing gold nanorods according to claim 6,
wherein a quaternary ammonium salt expressed by the following expression [I] is used as the surfactant.
CH3(CH2)nN+(CH3)3Br− (n=integer of 1 to 15) [I]

### Claim at position 9

11-20. (canceled)

### Claim 21 (depends on 3)

A coating composition, a coating or a film comprising the gold nanorods manufactured using the method according to claim 3.

### Claim 22 (depends on 3)

A wiring material, an electrode material, a catalyst, a colorant, a cosmetic, a near infra red absorber, anti-counterfeit ink, an electromagnetic shielding material, a surface enhanced fluorescent sensor, a biomarker or a nano-waveguide comprising the gold nanorods manufactured using the method according to claim 3.

### Claim 23 (depends on 7)

The method for manufacturing gold nanorods according to claim 7, wherein a quaternary ammonium salt expressed by the following expression [I] is used as the surfactant.
CH3(CH2)nN+(CH3)3Br (n=integer of 1 to 15) [I]

### Claim 24 (depends on 4)

A coating composition, a coating or a film comprising the gold nanorods manufactured using the method according to claim 4.

### Claim 25 (depends on 4)

A wiring material, an electrode material, a catalyst, a colorant, a cosmetic, a near-infra red absorber, anti-counterfeit ink, an electromagnetic shielding material, a surface enhanced fluorescent sensor, a biomarker or a nano-waveguide comprising the gold nanorods manufactured using the method according to claim 4.