# US 2010/0071811 A1 · AMORPHOUS Fe100-a-bPaMb ALLOY FOIL AND METHOD FOR ITS PREPARATION

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2010/0071811 A1
- Document ID: US20100071811A1
- Status: Published application
- Kind: A1
- Application number: 12/525,286
- Filed: 2008-02-01
- Published: 2010-03-25
- Earliest claimed: 2007-02-02
- Assignees: Hydro-Quebec
- Inventors: Robert Lacasse; Estelle Potvin; Michel Trudeau; Julian Cave; Francois Allaire; Georges Houlachi
- Web page: https://patentgrep.com/patent/US20100071811A1

## CPC

- C25C 1/24: Alloys obtained by cathodic reduction of all their ions
- C22C 45/02: with iron as the major constituent
- C25D 1/04: Wires; Strips; Foils
- C25D 3/562: {containing more than 50% by weight of iron or nickel or cobalt}
- C25D 5/18: Electroplating using modulated, pulsed or reversing current
- C25D 5/48: After-treatment of electroplated surfaces
- C25D 5/619: {Amorphous layers}
- C25D 5/625: {Discontinuous layers, e.g. microcracked layers}
- H01F 1/15308: {based on Fe/Ni (H01F1/15325 takes precedence)}
- H01F 1/15333: {containing nanocrystallites, e.g. obtained by annealing}
- H01F 41/26: using electric currents {, e.g. electroplating}
- H01F 41/0226: {from amorphous ribbons}
- C25C: PROCESSES FOR THE ELECTROLYTIC PRODUCTION, RECOVERY OR REFINING OF METALS; APPARATUS THEREFOR
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C25D: PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR
- H01F: MAGNETS; INDUCTANCES; TRANSFORMERS; SELECTION OF MATERIALS FOR THEIR MAGNETIC PROPERTIES

## Abstract

Amorphous Fe100-a-bPaMb foil, preferably in the form of a free-standing foil, process for its production by electrodeposition or electroforming of an aqueous plating solution, and its uses as a constitutive element of a transformer, generator, motor, pulse applications and magnetic shieldings. “a” is a real number ranging from 13 to 24, b is a real number ranging from 0 to 4, and M is at least one transition element other than Fe. The amorphous Fe100-a-bPaMb foil has the properties of being amorphous as established by the X-ray diffraction method, an average thickness greater than 20 micrometers, a tensile strength in the range of 200-1100 MPa, an electrical resistivity of over 120 μΩcm, and at least one of a high saturation induction (Bs) greater than 1.4 T, a coercive field (Hc) of less than 40 A/m, a loss (W60), at power frequencies (60 Hz), and for a peak induction of at least 1.35 T, of less than 0.65 W/kg, and a relative magnetic permeability (B/μ0H) greater than 10000, for low values of μ0H,

## Claims

### Claim at position 1

1-44. (canceled)

### Claim 45

A method for the preparation of an amorphous Fe100-a-bPaMb alloy, in the form of a free-standing foil, wherein:
said foil has an average thickness in the range 20 μm-250 μm;
in formula Fe100-a-bPaMb, a is a number ranging from 13 to 24, b is a real number ranging from 0 to 4, and M is at least one transition element other than Fe;
the alloy has an amorphous matrix in which nanocrystals having a size lower than 20 nm may be embedded, and the amorphous matrix occupies more than 85% of the volume of the alloy,
wherein
said method comprises electrodeposition using an electrochemical cell having a working electrode which is the substrate for the alloy deposition and an anode,
said electrochemical cell contains an electrolyte solution which acts as a plating solution and a dc current or a pulse current is applied between the working electrode and the anode,
the plating solution is an aqueous solution with a pH ranging from 0.8 to 2.5 and a temperature ranging from 40° C. to 105° C., which contains:
an iron precursor, preferably at a concentration ranging from 0.5 to 2 M, selected from the group consisting of a clean iron scrap, iron, pure iron, and a ferrous salt, said ferrous salt preferably selected in the group consisting of FeCl2, Fe(SO3NH2)2, FeSO4 and mixtures thereof;
a phosphorus precursor, preferably selected in the group consisting of NaH2PO2, H3PO2, H3PO3, and mixtures thereof, at a concentration ranging from 0.035-1.5 M; and
optionally a M salt at a concentration ranging from 0.1 to 500 mM;
a dc or pulse current is applied between the working electrode and the anode with a density ranging from 3 to 150 A/dm2;
wherein the working electrode and the anode are static parallel plate electrodes, and the velocity of the aqueous plating solution is of the order of 100 to 320 cm/s and the gap between the static parallel electrodes is from 0.3 cm to 3 cm.

### Claim 46 (depends on 45)

A method according to claim 45, which further comprises a step of peeling the alloy deposit from the working electrode.

### Claim 47 (depends on 45)

A method according to claim 45, wherein the pH of the aqueous plating solution is adjusted during its preparation by addition of at least one acid and/or at least one base.

### Claim 48 (depends on 45)

A method according to claim 45, wherein the ferric ion concentration in the aqueous plating solution is maintained at a low level by reducing ferric ions by recirculating the aqueous plating solution in a chamber so-called regenerator, containing iron chips.

### Claim 49 (depends on 45)

A method according to claim 45, which is carried out in the absence of oxygen, and preferably in the presence of an inert gas.

### Claim 50 (depends on 45)

A method according to claim 45, wherein the anode in the electrochemical cell is made of iron or graphite or DSA (Dimensionally Stabilized Anode).

### Claim 51 (depends on 45)

A method according to claim 45, wherein the anode has at least the same surface dimension as the working electrode.

### Claim 52 (depends on 45)

A method according to claim 45, wherein the anode is made of iron, and is isolated from the working electrode by a porous membrane.

### Claim 53 (depends on 45)

A method according to claim 45, wherein the working electrode is made of an electroconductive metal or metallic alloy.

### Claim 54 (depends on 53)

A method according to claim 53, wherein the working electrode is made of titanium, brass, hard chrome plated stainless steel or stainless steel.

### Claim 55 (depends on 54)

A method according to claim 54, wherein the working electrode is made of titanium and is polished before use.

### Claim 56 (depends on 45)

A method according to claim 45, wherein the temperature of the aqueous plating solution ranges from 40 to 60° C., and:
the concentration of the iron precursors is about 1 M;
the aqueous plating solution contains phosphorus precursor with a concentration ranging from 0.035 to 0.12 M;
the pH of the plating solution is from 1.2 to 1.4; and
the current may be a direct current or a pulse reverse current.

### Claim 57 (depends on 56)

A method according to claim 56, wherein the current is:
a direct current having a current density from 3 to 20 A/dm2; or
a pulse reverse current having a reductive current density from 3 to 20 A/dm2 at pulse interval of about 10 msec and a reverse current density of about 1 A/dm2 for an interval of 1-5 millisec.

### Claim 58 (depends on 45)

A method according to claim 45, wherein the temperature of the aqueous plating solution ranges from 60 to 85° C., and
the reducing current has a current density from 20 to 80 A/dm2;
the pH of the plating solution is maintained between 0.9 to 1.2; and
the concentration of the iron salts is about 1 M and the phosphorus precursor concentration is ranging from 0.12 to 0.5 M.

### Claim 59 (depends on 45)

A method according to claim 45, wherein the temperature of the plating solution ranges from 85 to 105° C., and
the reducing current has a current density of 80 to 150 A/dm2;
the concentration of the iron salts is of 1 to 1.5 M and the phosphorus precursor concentration is 0.5 to 0.75 M; and
the pH of the solution is maintained between 0.9 to 1.2.

### Claim 60 (depends on 45)

A method according to claim 45, comprising an additional step of thermal treatment of the amorphous Fe100-a-bPaMb foil, said additional step being performed at a temperature ranging from 200 to 300° C. with or without the presence of an applied magnetic field.

### Claim 61 (depends on 45)

A method according to claim 45, comprising an additional step of mechanical or chemical polishing of the amorphous Fe100-a-bPaMb foil.

### Claim 62 (depends on 45)

A method according to claim 45, comprising an additional surface treatment, said additional surface treatment being a laser treatment.

### Claim 63 (depends on 45)

A method according to claim 45, wherein additives, are added during the method, wherein said additives are selected from:
a complexing agent for inhibiting ferrous ions oxidation, selected from ascorbic acid, glycerine, (3-alanine, citric acid, and gluconic acid;
an agent for reducing the ferric ions, selected from hydroquinone and hydrazine; or
anti-stress additives for reducing stress in the foil, said additives being as sulphur containing organic additives and/or as aluminium derivatives, such as Al(OH)3,
at least one of this additive being preferably added in the step of preparation of the aqueous plating solution.

### Claim 64 (depends on 45)

An amorphous alloy Fe100-a-bPaMb alloy, in the form of a free-standing foil obtained by a method according to claim 45, wherein:
said foil has an average thickness in the range 20 μm-250 μm;
in formula Fe100-a-bPaMb, a is a number ranging from 13 to 24, b is a real number ranging from 0 to 4, and M is at least one transition element other than Fe; and
the alloy has an amorphous matrix in which nanocrystals having a size lower than 20 nm may be embedded, and the amorphous matrix occupies more than 85% of the volume of the alloy.

### Claim 65 (depends on 64)

An amorphous alloy according to claim 64, wherein the nanocrystals have a size lower than 5 nm.

### Claim 66 (depends on 64)

An amorphous alloy according to claim 64, wherein the amorphous matrix occupies 100% of the volume of the alloy.

### Claim 67 (depends on 64)

An amorphous alloy according to claim 64, having a tensile strength in the range of 200-1100 MPa, and a low hysteresis loss (W60) of less than 0.65 W/kg at power frequencies (60 Hz) and for a peak induction of at least 1.35 T.

### Claim 68 (depends on 64)

An amorphous alloy according to claim 64, wherein M is a single element selected in the group consisting of Mo, Mn, Cu, V, W, Cr, Cd, Ni, Co, Zn and or combination of at least two of said elements.

### Claim 69 (depends on 45)

An amorphous alloy according to claim 45, wherein M is Cu, Mn, Mo or Cr.

### Claim 70 (depends on 64)

An amorphous alloy according to claim 64, which contains less than 1% of one or more elements selected from oxygen, hydrogen, sodium, calcium, carbon, electrodeposited metallic impurities other than Mo, Mn, Cu, V, W, Cr, Cd, Ni, Co, or Zn.

### Claim 71 (depends on 64)

An amorphous alloy according to claim 64, wherein the alloy has one of the following formulae:
Fe100-a-b′PaCub′, or Fe100-a-b′PaMnb′, wherein a ranges from 15 to 21, and b′ ranges from 0.2 to 1.6;
Fe100-a-b″PaMob″, or Fe100-a-b″PaCrb″, wherein a ranges from 15 to 21, and b″ ranges from 0.5 to 3.
Fe100-a-bPaMb wherein Mb is Cub′Mob″, Cub′Crb″, Mnb′Mob″, or Mnb′Crb″; i.e. formulae Fe100-a-b′-b″PaCub′Mob″, Fe100-a-b′-b″PaCub′Crb Fe100-a-b′-b″PaMnb′Mob or Fe100-a-b′-b″PaMnb′Crb, wherein a ranges from 15 to 21; c′ ranges from 0.2 to 1.6; and c″ ranges from 0.5 to 3.

### Claim 72 (depends on 67)

An amorphous alloy according to claim 67, wherein the hysteresis loss (W60) is from 0.39 to 0.434 W/kg, at power frequencies (60 Hz), and for a peak induction of at least 1.35 T.

### Claim 73 (depends on 64)

Use of an amorphous Fe100-a-bPaMb foil according to claim 64 as a constitutive element of a transformer, a generator, a motor for frequencies ranging from about 1 Hz to 1000 Hz, for pulse applications and as magnetic shieldings.