# US 2009/0269608 A1 · Al-Zn-Mg-Cu ALLOY WITH IMPROVED DAMAGE TOLERANCE-STRENGTH COMBINATION PROPERTIES

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2009/0269608 A1
- Document ID: US20090269608A1
- Status: Published application
- Kind: A1
- Application number: 12/497,987
- Filed: 2009-07-06
- Published: 2009-10-29
- Earliest claimed: 2003-04-10
- Assignees: Aleris Aluminum Koblenz GmbH
- Inventors: Rinze Benedictus; Christian Joachim Keidel; Alfred Ludwig Heinz; Nedia Telioui
- Web page: https://patentgrep.com/patent/US20090269608A1

## CPC

- C22F 1/053: of alloys with zinc as the next major constituent
- C22C 21/10: with zinc as the next major constituent
- Y10T 428/12: All metal or with adjacent metals
- Y10T 428/12389: having variation in thickness
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- Y10T: TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION

## Abstract

An Al—Zn—Mg—Cu alloy with improved damage tolerance-strength combination properties. The present invention relates to an aluminium alloy product comprising or consisting essentially of, in weight %, about 6.5 to 9.5 zinc (Zn), about 1.2 to 2.2% magnesium (Mg), about 1.0 to 1.9% copper (Cu), preferable (0.9Mg−0.6)≦Cu≦(0.9Mg+0.05), about 0 to 0.5% zirconium (Zr), about 0 to 0.7% scandium (Sc), about 0 to 0.4% chromium (Cr), about 0 to 0.3% hafnium (Hf), about 0 to 0.4% titanium (Ti), about 0 to 0.8% manganese (Mn), the balance being aluminium (Al) and other incidental elements. The invention relates also to a method of manufacturing such as alloy.

## Claims

### Claim 1

An aluminium alloy product with high strength and fracture toughness and a good corrosion resistance, said alloy consisting of, in weight %:
Zn
7.2 to 7.9
Mg
1.92 to 2.1
Cu
1.43 to 1.80
Zr
0.04 to 0.15
Ti
<0.05
Fe
<about 0.08
Si
<about 0.07
Mn
at most 0.19,
and other impurities or incidental elements each <0.05, total <0.15, and the balance being aluminium.

### Claim 2 (depends on 1)

Aluminium alloy product according to claim 1, wherein Mg is in a range of 1.92 to 1.95.

### Claim 3 (depends on 1)

Aluminium alloy product according to claim 1, wherein
Mg is in a range of 1.92 to 1.95
Cu is in a range of 1.43 to 1.75.

### Claim 4 (depends on 1)

Aluminium alloy product according to claim 1, wherein the Zn-content is in a range of 7.2 to 7.7%.

### Claim 5 (depends on 1)

Aluminium alloy product according to claim 1, wherein the Zn-content is in a range of 7.2 to 7.43%.

### Claim 6 (depends on 1)

Aluminium alloy product according to claim 1, wherein the Zr-content is at least 0.06% to 0.15.

### Claim 7 (depends on 1)

Aluminium alloy product according claim 1, wherein
the Zr-content is in a range of 0.04 to 0.13%.

### Claim 8 (depends on 1)

Aluminium alloy product according to claim 1, wherein
the Zr-content is in a range of 0.04 to 0.11%.

### Claim 9 (depends on 1)

Aluminium alloy product according claim 1, wherein the Zr-content is in a range of about 0.06 to 0.15%.

### Claim 10 (depends on 1)

Aluminium alloy product according claim 1, wherein the Zr-content is in a range of about 0.06 to 0.01%.

### Claim 11 (depends on 1)

Aluminium alloy product according to claim 1, wherein the Mn-content is in a range <0.11%.

### Claim 12 (depends on 1)

Aluminium alloy product according to claim 1, wherein the Mn-content is in a range of at most 0.02%.

### Claim 13 (depends on 1)

Aluminium alloy product according to claim 1, wherein the Mn-content is in a range of at most 0.01%.

### Claim 14 (depends on 1)

Aluminium alloy product according to claim 1, wherein the alloy product is substantially free from Mn.

### Claim 15 (depends on 1)

Aluminium alloy product according to claim 1, wherein the alloy consists essentially of, in weight percent:
Zn
7.2 to 7.7
Mg
1.90 to 1.97
Cu
1.43 to 1.80
Zr
0.04 to 0.15
Mn
at most 0.19
Si
<0.07
Fe
<0.08
Ti
<0.05,
impurities each <0.05, total <0.15, and balance aluminium.

### Claim 16 (depends on 1)

Aluminium alloy product according to claim 1, wherein the alloy consists essentially of, in weight percent:
Zn
7.2 to 7.7
Mg
1.90 to 1.97
Cu
1.43 to 1.52
Zr
0.04 to 0.15
Mn
at most 0.19
Si
<0.07
Fe
<0.08
Ti
<0.05,
impurities each <0.05, total <0.15, and balance aluminium.

### Claim 17 (depends on 1)

Aluminium alloy product according to claim 1, wherein the product has an EXCO corrosion resistance of “EB” or better.

### Claim 18 (depends on 1)

Aluminium alloy product according to claim 1, wherein the product has an EXCO corrosion resistance of “EA” or better.

### Claim 19 (depends on 1)

Aluminium alloy product according to claim 1, wherein the product is in the form of a sheet, plate, forging or extrusion.

### Claim 20 (depends on 1)

Aluminium alloy product according to claim 1, wherein the product is in the form of a sheet, plate forging, or extrusion as part of an aircraft structural part.

### Claim 21 (depends on 1)

Aluminium alloy product according to claim 1, wherein the product is fuselage sheet, upper wing plate, lower wing plate, thick plate for machined parts, forging or thin sheet for stringers.

### Claim 22 (depends on 1)

Aluminium alloy product according to claim 1, wherein the product has a thickness in the range of 0.7 to 3 inch at its thickest cross sectional point.

### Claim 23 (depends on 1)

Aluminium alloy product according to claim 1, wherein the product has a thickness of less than 1.5 inch.

### Claim 24 (depends on 35)

Aluminium alloy product according to claim 35, wherein the product has a thickness of less than 1.0 inch.

### Claim 25 (depends on 1)

Aluminium alloy product according to claim 1, wherein the product has a thickness of more than 2.5 inch.

### Claim 26 (depends on 37)

Aluminium alloy product according to claim 37, wherein the product has a thickness in the range of 2.5 to 11 inch.

### Claim 27 (depends on 1)

Aluminium alloy product according to claim 1, which in an extrusion having a thickness in the range of at most 10 mm at its thickest cross sectional point.

### Claim 28 (depends on 1)

Aluminium alloy product according to claim 1, which is an extrusion having a thickness in the range of 2 to 6 inch at its thickest cross sectional point.

### Claim 29 (depends on 1)

Aluminium alloy product according to claim 1, wherein the product is in the form of a sheet or plate.

### Claim 30 (depends on 1)

Aluminium alloy product according to claim 1, wherein the product is in the form of a forging or extrusion.

### Claim 31 (depends on 30)

Aluminium alloy product according to claim 30, wherein the product has a thickness of more than 2.5 inch.

### Claim 32 (depends on 1)

Aluminium alloy product according to claim 1, wherein the product is fuselage sheet, upper wing plate, lower wing plate, thick plate for machined parts, forging or thin sheet for stringers.

### Claim 33 (depends on 1)

Aluminium alloy product according to claim 1, which in an extrusion having a thickness in the range of at most 10 mm at its thickest cross sectional point.

### Claim 34 (depends on 1)

Aluminium alloy product according to claim 1, which is a plate product having a thickness of 2.5 inch or more and exhibiting increased elongation in the ST-testing direction compared to its AA7050 counterpart.

### Claim 35 (depends on 34)

Aluminium alloy product according to claim 34, which plate product has an elongation in the ST-testing direction of 5% or more.

### Claim 36 (depends on 34)

Aluminium alloy product according to claim 34, which plate product has an elongation in the ST-testing direction of 5.5% or more.

### Claim 37 (depends on 1)

Aluminium alloy product according to claim 1, which is a plate product having a thickness of 2.5 inch or more and exhibiting a fracture toughness Kapp improvement of at least 20% compared to its AA7050 aluminium alloy counterpart in the L-T testing direction at ambient room temperature and when measured at S/4 according to ASTM E561 using 16-inch centre cracked panels.

### Claim 38 (depends on 1)

Aluminium alloy product according to claim 1, which is a plate product having a thickness of 2.5 inch or more and exhibiting a fracture toughness Kapp improvement of at least 20% compared to its AA7050 aluminium alloy counterpart in the L-T testing direction at ambient room temperature and when measured at S/4 according to ASTM E561 using 16-inch centre cracked panels.

### Claim 39 (depends on 1)

Method of producing a high-strength, high-toughness AA7xxx-series alloy product having a good corrosion resistance comprising the processing steps of:
a) casting an ingot having a composition according to claim 1;
b) homogenising and/or pre-heating the ingot after casting;
c) hot working the ingot into a pre-worked product by one or more methods selected from the group consisting of: rolling, extruding and forging;
d) optionally reheating the pre-worked product and either;
e) hot working and/or cold working to a desired workpiece form;
f) solution heat treating said formed workpiece at a temperature and time sufficient to place into solid solution essentially all soluble constituents in the alloy;
g) quenching the solution heat treated workpiece by one of spray quenching or immersion quenching in water or other quenching media;
h) optionally stretching or compressing of the quenched workpiece;
i) artificially ageing the quenched and optionally stretched or compressed workpiece to achieve a desired temper.

### Claim 40 (depends on 39)

Method according to claim 39, wherein during processing step i) the alloy product is artificially aged to a temper selected from the group consisting of T6, T74, T76, T751, T7451, T7651, T77 and T79.

### Claim 41 (depends on 39)

Method according to claim 39, wherein during processing step h.) the alloy product has been stretched in a range at most 8%.

### Claim 42 (depends on 39)

Method according to claim 39, wherein during processing step b) the ingot has been homogenized at a temperature in the range of 460 to 490° C.

### Claim 43 (depends on 39)

Method according to claim 39, wherein the alloy product has been processed to fuselage sheet.

### Claim 44 (depends on 43)

Method according to claim 43, wherein the alloy product has been processed to fuselage sheet having a thickness of less than 1.5 inch.

### Claim 45 (depends on 39)

Method according to claim 39, wherein the alloy product has been processed to lower wing plate.

### Claim 46 (depends on 39)

Method according to claim 39, wherein the alloy products has been processed to upper wing plate.

### Claim 47 (depends on 39)

Method according to claim 39, wherein the alloy product has been processed to an extruded product.

### Claim 48 (depends on 39)

Method according to claim 39, wherein the alloy product has been processed to a forged product.

### Claim 49 (depends on 39)

Method according to claim 39, wherein the alloy product has been processed to a thin plate having a thickness in the range of 0.7 to 3 inch.

### Claim 50 (depends on 39)

Method according to claim 39, wherein the alloy product has been processed to a thick plate having a thickness at most 11 inch.

### Claim 51 (depends on 16)

Method of producing a high-strength, high-toughness AA7xxx-series alloy product having a good corrosion resistance, comprising the processing steps of:
a) casting an ingot having a composition according to claim 16;
b) homogenising and/or pre-heating the ingot after casting;
c) hot working the ingot into a pre-worked product by one or more methods selected from the group consisting of: rolling, extruding and forging;
d) optionally reheating the pre-worked product and either;
e) hot working and/or cold working to a desired workpiece form;
f) solution heat treating said formed workpiece at a temperature and time sufficient to place into solid solution essentially all soluble constituents in the alloy;
g) quenching the solution heat treated workpiece by one of spray quenching or immersion quenching in water or other quenching media;
h) optionally stretching or compressing of the quenched workpiece;
i) artificially ageing the quenched and optionally stretched or compressed workpiece to achieve a desired temper.

### Claim 52 (depends on 51)

Method according to claim 51, wherein during processing step i.) the alloy product is artificially aged to a temper selected from the group consisting of T6, T74, T76, T751, T7451, T7651, T77 and T79.

### Claim at position 53

53-123. (canceled)