# US 2008/0305258 A1 · Method for forming dielectric film using porogen gas

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2008/0305258 A1
- Document ID: US20080305258A1
- Status: Published application
- Kind: A1
- Application number: 11/759,439
- Filed: 2007-06-07
- Published: 2008-12-11
- Earliest claimed: 2007-06-07
- Assignees: ASM Japan K.K.
- Inventors: Naoto TSUJI
- Web page: https://patentgrep.com/patent/US20080305258A1

## CPC

- C23C 16/401: {containing silicon}
- C23C 16/56: After-treatment
- H10P 14/6538: {by exposure to UV light}
- H10P 14/6336: {in the presence of a plasma [PECVD]}
- H10P 14/665: {Porous materials}
- H10P 14/6686: {the compound being a molecule comprising at least one silicon-oxygen bond and the compound having hydrogen or an organic group attached to the silicon or oxygen, e.g. a siloxane}
- H10P 14/6922: {the material containing Si, O and at least one of H, N, C, F or other non-metal elements, e.g. SiOC, SiOC:H or SiONC}
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- H10P: GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10

## Abstract

A method for reducing a dielectric constant of a cured film, includes: introducing a source gas at a flow rate of A, a porogen gas at a flow rate of B, an oxidizing gas at a flow rate of C, and an inert gas into a reaction space in which a substrate is place; increasing a ratio of B/(A+B) used as a parameter for controlling a dielectric constant of a cured film, by a degree substantially or nearly in proportion to a target decrease of dielectric constant of a cured film; applying RF power to the reaction space, thereby depositing a film on the substrate by plasma CVD; and curing the film to remove the porogen material, thereby forming pores in the cured film.

## Claims

### Claim 1

A method for reducing a dielectric constant of a cured film, comprising:
introducing a source gas at a flow rate of A, a porogen gas at a flow rate of B, an oxidizing gas at a flow rate of C, and an inert gas into a reaction space in which a substrate is place, said source gas being a silicon-containing hydrocarbon compound having multiple cross linkable groups, said porogen gas being a gas constituted by a porogen material;
increasing a ratio of B/(A+B) used as a parameter for controlling a dielectric constant of a cured film, by a degree substantially or nearly in proportion to a target decrease of dielectric constant of a cured film;
applying RF power to the reaction space, thereby depositing a film on the substrate by plasma CVD; and
curing the film to remove the porogen material, thereby forming pores in the cured film.

### Claim 2 (depends on 1)

The method according to claim 1, wherein the ratio of B/(A+B) is controlled in the range of 0.30-0.70, and the oxidizing gas is used to satisfy C/(A+B+C)=0.09-0.18, whereby as a result of the curing, the cured film has a dielectric constant of 2.4-2.7.

### Claim 3 (depends on 1)

The method according to claim 1, wherein the ratio of B/(A+B) is controlled in the range of 0.70-0.85, and the oxidizing gas is used to satisfy C/(A+B+C)=0.05-0.09, whereby as a result of the curing, the cured film has a dielectric constant of 2.1-2.4.

### Claim 4 (depends on 1)

The method according to claim 1, wherein the ratio of B/(A+B) is used as a single parameter for controlling a dielectric constant of the cured film.

### Claim 5 (depends on 1)

The method according to claim 1, wherein the porogen gas is constituted by at least one porogen material selected from the group consisting of straight-chain or branched or cyclic hydrocarbons having a formula CnHm wherein n is 4-14, and m is 4-30.

### Claim 6 (depends on 1)

The method according to claim 1, wherein the porogen material is selected from the group consisting of α-terpinene, β-terpinene, γ-terpinene, cyclohexane, and hexane.

### Claim 7 (depends on 6)

The method according to claim 6, wherein the porogen gas is constituted by α-terpinene, β-terpinene, or γ-terpinene.

### Claim 8 (depends on 1)

The method according to claim 1, wherein the reaction space for depositing the film is controlled at a temperature of higher than 200° C. but lower than 350° C.

### Claim 9 (depends on 1)

The method according to claim 1, further comprising, prior to the step of introducing gases:
establishing a relationship between B/(A+B) and dielectric constant of a cured film, which is substantially or nearly a linear inverse relationship, by:
(i) introducing a source gas at a flow rate of A, a porogen gas at a flow rate of B, an oxidizing gas, and an inert gas into a reaction space in which a substrate is place, said source gas being a silicon-containing hydrocarbon compound having multiple cross linkable groups, said porogen gas being a gas constituted by a porogen material;
(ii) changing a ratio of B/(A+B) used as a parameter for controlling a dielectric constant of a cured film;
(iii) applying RF power to the reaction space, thereby depositing a film on the substrate by plasma CVD;
(iv) curing the film to remove the porogen material, thereby forming pores in the film; and
(v) repeating steps (i) to (iv),
wherein in the step of increasing the ratio of B/(A+B), the ratio of B/(A+B) is determined according to a target decrease of dielectric constant of the cured film based on the established relationship.

### Claim 10 (depends on 1)

The method according to claim 1, wherein the cross linkable groups of the source gas are alkoxyl group and/or vinyl group.

### Claim 11 (depends on 10)

The method according to claim 10, wherein the source gas is constituted by at least one compound having a formula SiαOα−1R2α+β2(OCnH2n+1)β wherein α is an integer of 1-3, β is an integer of 2 or 3, n is an integer of 1-3, R is attached to Si has C1-12.

### Claim 12 (depends on 11)

The method according to claim 11, wherein α is 1 or 2, and β is 2.

### Claim 13 (depends on 1)

The method according to claim 1, wherein the oxidizing gas is O2 and/or N2O.

### Claim 14 (depends on 1)

The method according to claim 1, wherein the inert gas is Ne, He, and/or Ar.

### Claim 15 (depends on 1)

The method according to claim 1, wherein the inert gas is introduced at a flow rate which is 5 times to 30 times greater than the flow rate of the source gas.

### Claim 16 (depends on 1)

The method according to claim 1, wherein the curing step is performed at a temperature of 0° C. to 450° C.

### Claim 17

A method for forming a film having a low dielectric constant, comprising:
introducing a source gas at a flow rate of A, a porogen gas at a flow rate of B, an oxidizing gas at a flow rate of C, and an inert gas into a reaction space in which a substrate is place, said source gas being a silicon-containing hydrocarbon compound having multiple cross linkable groups, said porogen gas being a gas constituted by a porogen material selected from the group consisting of α-terpinene, β-terpinene, γ-terpinene, cyclohexane, and hexane, wherein B/(A+B) is 0.30-0.70 when C/(A+B+C) is 0.09-0.18, or B/(A+B) is 0.70-0.85 when C/(A+B+C) is 0.05-0.09;
applying RF power to the reaction space, thereby depositing a film on the substrate by plasma CVD; and
curing the film to remove the porogen material, thereby forming pores in the cured film.

### Claim 18 (depends on 17)

The method according to claim 17, wherein in the step of introducing gases, B/(A+B) is 0.30-0.70, and C/(A+B+C) is 0.09-0.18, and as a result of the curing, the cured film has a dielectric constant of 2.4-2.7.

### Claim 19 (depends on 18)

The method according to claim 18, wherein in the step of introducing gases, B/(A+B) is 0.70-0.85, and C/(A+B+C) is 0.05-0.09, and as a result of the curing, the cured film has a dielectric constant of 2.1-2.4.

### Claim 20

A method for controlling a dielectric constant of a cured film, comprising:
(i) introducing a source gas at a flow rate of A, a porogen gas at a flow rate of B, an oxidizing gas, and an inert gas into a reaction space in which a substrate is place, said source gas being a silicon-containing hydrocarbon compound having multiple cross linkable groups, said porogen gas being a gas constituted by a porogen material;
(ii) changing a ratio of B/(A+B) used as a parameter for controlling a dielectric constant of a cured film;
(iii) applying RF power to the reaction space, thereby depositing a film on the substrate by plasma CVD;
(iv) curing the film to remove the porogen material, thereby forming pores in the film;
(v) repeating steps (i) to (iv) to establish a relationship between B/(A+B) and dielectric constant of the cured film, which is substantially or nearly a linear inverse relationship; and
(vi) performing steps (i) to (iv) for a new substrate wherein in step (ii), the ratio of B/(A+B) is determined according to a target decrease of dielectric constant of a cured film based on the relationship established in step (v).