# US 2007/0261607 A1 · Fiber reinforced cement composition and products and manufacturing process

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2007/0261607 A1
- Document ID: US20070261607A1
- Status: Published application
- Kind: A1
- Application number: 11/431,652
- Filed: 2006-05-11
- Published: 2007-11-15
- Earliest claimed: 2006-05-11
- Assignees: Nichiha Corporation
- Inventors: Kazuo Utagaki; Tadashi Sugita; Satoshi Takayama
- Web page: https://patentgrep.com/patent/US20070261607A1

## CPC

- C04B 18/26: Wood, e.g. sawdust, wood shavings
- C04B 28/04: Portland cements
- Y02W 30/91: Use of waste materials as fillers for mortars or concrete
- Y10S 106/01: Fly ash
- Y10S 106/02: Perlite
- Y10S 106/03: Mica
- C04B: LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE {(roofing granules E04D7/005)}; CERAMICS (devitrified glass-ceramics C03C10/00); REFRACTORIES; TREATMENT OF NATURAL STONE
- Y02W: CLIMATE CHANGE MITIGATION TECHNOLOGIES RELATED TO WASTEWATER TREATMENT OR WASTE MANAGEMENT
- Y10S: TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS

## Abstract

The present invention relates to a fiber reinforced cement composition and products and a manufacturing process thereof. The fiber reinforced cement product and the manufacturing process are safe for human body, and, even more particularly, bending strength and dimensional stability and construction characteristics such as nail performance of the product are preferable. In other words, the fiber reinforced cement composition comprising a hydraulic inorganic material, a siliceous material and woody reinforcement, wherein a siliceous material is amorphous material.

## Claims

### Claim 1

A fiber reinforced cement composition comprising the following raw materials: a hydraulic inorganic material, a siliceous material and woody reinforcement, wherein a siliceous material is amorphous material.

### Claim 2 (depends on 1)

The fiber reinforced cement composition according to claim 1, wherein the siliceous material is fly ash and/or silica fume and/or blast furnace slag and/or perlite powder and/or glass powder.

### Claim 3 (depends on 1)

The fiber reinforced cement composition according to claim 1, wherein the siliceous material is fly ash which contains not less than 50% by mass and not more than 70% by mass of SiO2 component.

### Claim 4 (depends on 1)

The fiber reinforced cement composition according to claim 1, wherein the siliceous material is silica fume which contains not less than 97% by mass of SiO2 component.

### Claim 5 (depends on 1)

The fiber reinforced cement composition according to claim 1, wherein the siliceous material is blast furnace slag which contains not less than 20% by mass and not more than 40% by mass of SiO2 component.

### Claim 6 (depends on 1)

The fiber reinforced cement composition according to claim 1, wherein the hydraulic inorganic material is a Portland cement.

### Claim 7 (depends on 1)

The fiber reinforced cement composition according to claim 1, wherein the hydraulic inorganic material is a Portland cement having the following chemical composition:
SiO2: not less than 18.0% by mass and not more than 23.0% by mass,
Al2O3: not less than 2.0% by mass and not more than 6.0% by mass,
Fe2O3: not less than 1.0% by mass and not more than 6.0% by mass,
CaO: not less than 60.0% by mass and not more than 65.0% by mass,
MgO: not more than 6.0% by mass,
SO3: not more than 3.0% by mass,
Na2O: not more than 0.3% by mass, and
K2O: not more than 0.7% by mass.

### Claim 8 (depends on 1)

The fiber reinforced cement composition according to claim 1, wherein the hydraulic inorganic material is a Portland cement comprising having the following mineralogical compositions;
C3S: not less than 60.0% by mass and not more than 65.0% by mass,
C2S: not less than 9.0% by mass and not more than 13.0% by mass,
C3A: not less than 5.0% by mass and not more than 9.0% by mass, and
C4AF: not less than 6.0% by mass and not more than 10.0% by mass.

### Claim 9 (depends on 1)

The fiber reinforced cement composition according to claim 1, wherein the woody reinforcement is NUKP and/or NBKP having a Canadian standard freeness of not more than 500 ml.

### Claim 10 (depends on 1)

The fiber reinforced cement composition according to claim 1, wherein the woody reinforcement is a used paper having a fiber length of not less than 0.5 mm and not more than 3.0 mm, a fiber diameter of not less than 10 μm and not more than 100 μm, and a Canadian standard freeness of not more than 350 ml.

### Claim 11 (depends on 1)

The fiber reinforced cement composition according to claim 1, wherein the woody reinforcement is a mixture of two kinds of woody reinforcement.

### Claim 12 (depends on 1)

The fiber reinforced cement composition according to claim 1, wherein the woody reinforcement is a mixture of NUKP and/or NBKP and used paper in a ratio of the NUKP and/or NBKP to the used paper in a range of from 1:1 to 4:1.

### Claim 13 (depends on 1)

The fiber reinforced cement composition according to claim 1 comprising the following raw material composition: not less than 25% by mass and not more than 45% by mass of the hydraulic inorganic material, not less than 50% by mass and not more than 65% by mass of the siliceous material, and not less than 5% by mass and not more than 12% by mass of the woody reinforcement.

### Claim 14 (depends on 13)

The fiber reinforced cement composition according to claim 13, additionally comprising mica in an amount of not less than 1% by mass and not more than 7% by mass of the composition.

### Claim 15 (depends on 13)

The fiber reinforced cement composition according to claim 13, additionally comprising a water-soluble resin in an amount of not less than 0.25% by mass and not more than 1.5% by mass of the composition.

### Claim 16 (depends on 13)

The fiber reinforced cement composition according to claim 13, additionally comprising mica in an amount of not less than 1% by mass and not more than 7% by mass and a water-soluble resin in an amount of not less than 0.25% by mass and not more than 1.5% by mass based on the composition.

### Claim 17

The fiber reinforced cement composition having the following raw material composition: not less than 28% by mass and not more than 32% by mass of Portland cement as hydraulic inorganic material, not less than 54% by mass and not more than 58% by mass in total of fly ash and silica fume as a amorphous siliceous material, wherein the amount of the silica fume is not less than 3% by mass and not more than 7% by mass of the whole amorphous siliceous material consisting of the fly ash and the silica fume, not less than 8% by mass and not more than 12% by mass in total of NUKP and/or NBKP and used paper as a woody reinforcement, wherein the amount of the used paper is not less than 20% by mass and not more than 50% by mass of the whole woody reinforcement consisting of the NUKP and/or NBKP and the used paper, not less than 2% by mass and not more than 5% by mass of mica, and not less than 0.5% by mass and not more than 1.25% by mass of a water-soluble resin.

### Claim 18

The fiber reinforced cement composition having the following raw material composition: not less than 28% by mass and not more than 32% by mass of Portland cement as hydraulic inorganic material, not less than 54% by mass and not more than 58% by mass in total of blast furnace slag and silica fume as a amorphous siliceous material, wherein the amount of the silica fume is not less than 5% by mass and not more than 20% by mass of the whole amorphous siliceous material consisting of the blast furnace slag and the silica fume, not less than 8% by mass and not more than 12% by mass in total of NUKP and/or NBKP and used paper as a woody reinforcement, wherein the amount of the used paper is not less than 20% by mass and not more than 50% by mass of the whole woody reinforcement consisting of the NUKP and/or NBKP and the used paper, not less than 2% by mass and not more than 5% by mass of mica, and not less than 0.5% by mass and not more than 1.25% by mass of a water-soluble resin.

### Claim 19

The fiber reinforced cement composition having the following raw material composition: not less than 28% by mass and not more than 32% by mass of Portland cement as hydraulic inorganic material, not less than 54% by mass and not more than 58% by mass in total of blast furnace slag and fly ash as a amorphous siliceous material, wherein the amount of the fly ash is not less than 30% by mass and not more than 70% by mass of the whole amorphous siliceous material consisting of the blast furnace slag and the fly ash, not less than 8% by mass and not more than 12% by mass in total of NUKP and/or NBKP and used paper as a woody reinforcement, wherein the amount of the used paper is not less than 20% by mass and not more than 50% by mass of the whole woody reinforcement consisting of the NUKP and/or NBKP and the used paper, not less than 2% by mass and not more than 5% by mass of mica, and not less than 0.5% by mass and not more than 1.25% by mass of a water-soluble resin.

### Claim 20 (depends on 17)

The fiber reinforced cement product manufactured from the fiber reinforced cement composition according to claim 17.

### Claim 21

The fiber reinforced cement product having the following physical property conditions: the product does not have the peak manifestation of crystalline silica in X-ray diffraction.

### Claim 22 (depends on 21)

The fiber reinforced cement product according to claim 21, having the following raw material composition: not less than 28% by mass and not more than 32% by mass of Portland cement as hydraulic inorganic material, not less than 54% by mass and not more than 58% by mass in total of fly ash and silica fume as a amorphous siliceous material, wherein the amount of the silica fume is not less than 3% by mass and not more than 7% by mass of the whole amorphous siliceous material consisting of the fly ash and the silica fume, not less than 8% by mass and not more than 12% by mass in total of NUKP and/or NBKP and used paper as a woody reinforcement, wherein the amount of the used paper is not less than 20% by mass and not more than 50% by mass of the whole woody reinforcement consisting of the NUKP and/or NBKP and the used paper, not less than 2% by mass and not more than 5% by mass of mica, and not less than 0.5% by mass and not more than 1.25% by mass of a water-soluble resin.

### Claim 23 (depends on 21)

The fiber reinforced cement product according to claim 21, having the following raw material composition: not less than 28% by mass and not more than 32% by mass of Portland cement as hydraulic inorganic material, not less than 54% by mass and not more than 58% by mass in total of blast furnace slag and silica fume as a amorphous siliceous material, wherein the amount of the silica fume is not less than 5% by mass and not more than 20% by mass of the whole amorphous siliceous material consisting of the blast furnace slag and the silica fume, not less than 8% by mass and not more than 12% by mass in total of NUKP and/or NBKP and used paper as a woody reinforcement, wherein the amount of the used paper is not less than 20% by mass and not more than 50% by mass of the whole woody reinforcement consisting of the NUKP and/or NBKP and the used paper, not less than 2% by mass and not more than 5% by mass of mica, and not less than 0.5% by mass and not more than 1.25% by mass of a water-soluble resin.

### Claim 24 (depends on 21)

The fiber reinforced cement product according to claim 21, having the following raw material composition: not less than 28% by mass and not more than 32% by mass of Portland cement as hydraulic inorganic material, not less than 54% by mass and not more than 58% by mass in total of blast furnace slag and fly ash as a amorphous siliceous material, wherein the amount of the fly ash is not less than 30% by mass and not more than 70% by mass of the whole amorphous siliceous material consisting of the blast furnace slag and the fly ash, not less than 8% by mass and not more than 12% by mass in total of NUKP and/or NBKP and used paper as a woody reinforcement, wherein the amount of the used paper is not less than 20% by mass and not more than 50% by mass of the whole woody reinforcement consisting of the NUKP and/or NBKP and the used paper, not less than 2% by mass and not more than 5% by mass of mica, and not less than 0.5% by mass and not more than 1.25% by mass of a water-soluble resin.

### Claim 25

A process for manufacturing a fiber reinforced cement product comprising the steps of: dispersing in water a raw material composition comprising as main raw materials a hydraulic inorganic material, a amorphous siliceous material and a woody reinforcement mixed to give a slurry of the raw materials; forming a green mat by forming the slurry; and pressing the green mat by press molding and thereafter curing the mat in an autoclave at a temperature not lower than 150° C.

### Claim 26 (depends on 18)

The fiber reinforced cement product manufactured from the fiber reinforced cement composition according to claim 18.

### Claim 27 (depends on 19)

The fiber reinforced cement product manufactured from the fiber reinforced cement composition according to claim 19.