# US 2006/0162825 A1 · Weldable steel building component and method for making same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2006/0162825 A1
- Document ID: US20060162825A1
- Status: Published application
- Kind: A1
- Application number: 10/535,306
- Filed: 2003-11-13
- Published: 2006-07-27
- Earliest claimed: 2002-11-19
- Assignees: Usinor
- Inventors: Jean Beguinot; Jean-Georges Brisson
- Web page: https://patentgrep.com/patent/US20060162825A1

## CPC

- C21D 1/18: Hardening (C21D1/02 takes precedence); Quenching with or without subsequent tempering (quenching devices C21D1/62)
- C22C 38/54: with boron
- C21D 9/46: for sheet metals
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

The invention concerns weldable steel building components whereof the chemical composition comprises, by weight: 0.10%≦C≦0.22%, 0.50%≦Si≦1.50%, AI≦0.9%, 0%≦Mn≦3%, 0%≦Ni≦5%, 0%≦Cr≦4%, 0%≦Cu≦1%, 0%≦Mo+W/2≦1.5%, 0.0005%≦B<0.010%, N≦0.025%, optionally at least one element selected among V, Nb, Ta, S et Ca, in contents less than 0.3%, and/or among Ti and Zr in contents not more than 0.5%, the rest being iron and impurities resulting from preparation, the aluminium, boron, titanium and nitrogen contents, expressed in thousandths of %, of said composition further satisfying the following relationship: B≦1/3×K+0.5, (1) with K=Min (I*; J*), I*=Max (0; I) and J*=Max (0; J), I=Min (N; N-0.29(Ti-5)), J=Min {N; 0.5 (N 0.52 AI+√j(N 0.52 AI)2+283)}, the silicon and aluminium contents of the composition additionally verifying the following conditions: if C>0.145, then Si+AI<0.95 and whereof the structure is bainitic, martensitic or martensitic/bainitic and further comprises 3 to 20% of residual austenite.

## Claims

### Claim 1

Weldable component of structural steel, characterized in that its chemical composition comprises, by weight:
0.10%≦C≦0.22%
0.50%≦Si≦1.50%
Al≦0.9%
0%≦Mn≦3%
0%≦Ni≦5%
0%≦Cr≦4%
0%≦Cu≦1%
0%≦Mo+W/2≦1.5%
0.0005%≦B≦0.010%
N≦0.025%
optionally at least one element selected from V, Nb, Ta, S and Ca, at contents of less than 0.3%, and/or from Ti and Zr at contents of less than or equal to 0.5%, the remainder being iron and impurities resulting from the production operation, the contents of aluminium, boron, titanium and nitrogen, expressed in thousandths of %, of the composition also satisfying the following relationship:
B
≥
1
3
×
K
+
0
⁢
,
⁢
5
⁢
,
(
1
)
with
K=Min (I*; J*)
I*=Max (0; I) and J*=Max (0; J)
I=Min (N; N-0.29(Ti-5))
J=Min (N; 0.5(N-0.52 Al+√{square root over ((N-0.52 Al)2+283)})),
the contents of silicon and aluminium of the composition also complying with the following conditions:
if C>0.145, then Si+Al<0.95
and whose structure is bainitic, martensitic or martensitic-bainitic and also comprises from 3 to 20% of residual austenite.

### Claim 2 (depends on 1)

Steel component according to claim 1, characterized in that its chemical composition also satisfies the following relationship:
1.1% Mn+0.7% Ni+0.6% Cr+1.5(% Mo+% W/2)≧1 (2)

### Claim 3 (depends on 2)

Steel component according to claim 2, characterized also in that its chemical composition satisfies the following relationship:
1.1% Mn+0.7% Ni+0.6% Cr+1.5(% Mo+% W/2)≧2 (2)

### Claim 4 (depends on 1)

Steel component according to claim 1, characterized in that its chemical composition also satisfies the following relationship:
% Cr+3(% Mo+% W/2)≧1.8.

### Claim 5 (depends on 4)

Steel component according to claim 4, characterized in that its chemical composition also satisfies the following relationship:
% Cr+3(% Mo+% W/2)≧2.0.

### Claim 6 (depends on 1)

Method for manufacturing a weldable steel component according to claim 1, characterized in that
the component is austenitized by heating at a temperature of from Ac3 to 1000° C., and it is then cooled to a temperature of less than or equal to 200° C., in such a manner that, at the core of the component, the rate of cooling between 800° C. and 500° C. is greater than or equal to the critical bainitic velocity,
optionally, tempering is effected at a temperature of less than or equal to Ac1.

### Claim 7 (depends on 6)

Method according to claim 6, characterized in that, at the core of the component, the cooling rate between 500° C. and a temperature of less than or equal to 200° C. is from 0.07° C./s to 5° C./s.

### Claim 8 (depends on 6)

Method according to claim 6, characterized in that tempering is effected at a temperature of less than 300° C. for a period of time of less than 10 hours, at the end of the cooling operation to a temperature of less than or equal to 200° C.

### Claim 9 (depends on 6)

Method according to claim 6, characterized in that no tempering is carried out at the end of the cooling operation to a temperature of less than or equal to 200° C.

### Claim 10 (depends on 1)

Method for manufacturing a weldable steel plate according to claim 1, the thickness of which is from 3 mm to 150 mm, characterized in that the plate is quenched, the cooling rate VR at the core of the component between 800° C. and 500° C. and the composition of the steel being such that:
1.1% Mn+0.7% Ni+0.6% Cr+1.5(% Mo+% W/2)+log VR≧5.5.

### Claim 11 (depends on 10)

Method for manufacturing a weldable steel plate according to claim 10, the thickness of which is from 3 mm to 150 mm, characterized, in addition, in that the plate is quenched, the cooling rate VR at the core of the component between 800° C. and 500° C. and the composition of the steel being such that:
1.1% Mn+0.7% Ni+0.6% Cr+1.5(% Mo+% W/2)+log VR≧6.