# US 2006/0157166 A1 · Method for making hardenable steel plates by firing, resulting steel plates

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2006/0157166 A1
- Document ID: US20060157166A1
- Status: Published application
- Kind: A1
- Application number: 10/531,264
- Filed: 2003-10-10
- Published: 2006-07-20
- Earliest claimed: 2002-10-14
- Assignees: Usinor
- Inventors: Joel Marsal; Fernande Kirch; Dominique Mescolini
- Web page: https://patentgrep.com/patent/US20060157166A1

## CPC

- C22C 38/02: containing silicon
- C21D 8/0226: {Hot rolling}
- C21D 8/0236: {Cold rolling}
- C21D 8/0273: {Final recrystallisation annealing}
- C21D 9/52: for wires; for strips {; for rods of unlimited length}
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)

## Abstract

The invention concerns a method for making hardenable steel plates by firing comprising: preparing a steel whereof the composition comprises, expressed in weight percent: 0.03=C=0.06, 0.50=Mn=1.10, 0.08:=Si=0.20, 0.015=Al=0.070, N=0.007, Ni=0.040, Cu=0.040, P=0.035, S=0.015, Mo=0.010, Ti=0.005; provided that it comprises boron in an amount such that 0.64=B/N=1.60 the rest consisting of iron and impurities resulting from production; casting a slab of said steel, then hot rolling of said slab to obtain a plate, the final rolling temperature being higher than the point Ar3; winding said plate at a temperature ranging between 500 and 700° C.; then cold rolling of said plate at a reduction rate ranging between 50 and 80%; continuous annealing heat treatment for a time interval less than 15 minutes; and strain hardening with a reduction rate ranging between 1.25 and 2.5%. The invention also concerns the hardenable plates and the parts obtainable therefrom.

## Claims

### Claim 1

A process for manufacturing bake hardening steel sheet comprising:
the smelting of a steel, the composition of which comprises, expressed in % by weight:
0.03≦C≦0.06
0.50≦Mn≦1.10
0.08≦Si≦0.20
0.015≦Al≦0.070
N≦0.007
Ni≦0.040
Cu≦0.040
P≦0.035
S≦0.015
Mo≦0.010
Ti≦0.005
it being understood that the steel also contains boron in an amount such that:
0.64
≤
B
N
≤
1.60
the balance of the composition consisting of iron and impurities resulting from the smelting;
the casting of a slab of this steel, this slab then being hot rolled in order to obtain a sheet, the end-of-rolling temperature being above that of the Ar3 point;
the coiling of said sheet at a temperature of between 500 and 700° C.; then
the cold rolling of said sheet with a reduction ratio of 50 to 80%;
a continuous annealing heat treatment which is carried out for a time of less than 15 minutes; and
a skin pass which is carried out with a reduction ratio of between 1.2 and 2.5%.

### Claim 2 (depends on 1)

The process as claimed in claim 1, characterized in that said continuous annealing heat treatment comprises:
a reheat of the steel until it reaches a temperature of between 750 and 850° C.;
an isothermal soak;
a first cooling operation down to a temperature of between 380 and 500° C.; and
an isothermal soak; and then
a second cooling operation down to the ambient temperature.

### Claim 3 (depends on 1, 2)

The process as claimed in either of claims 1 and 2, characterized in that said first cooling operation comprises a slow first part carried out at a rate of less than 10° C./s, followed by a rapid second part carried out at a rate of between 20 and 50° C./s.

### Claim 4 (depends on 1, 2, 3)

The process as claimed in any one of claims 1 to 3, characterized in that, in addition, the manganese content and the silicon content of the steel are such that:
4
≤
%
⁢
⁢
Mn
%
⁢
⁢
Si
≤
15.

### Claim 5 (depends on 1, 2, 3, 4)

The process as claimed in any one of claims 1 to 4, characterized in that, in addition, the manganese content of the steel is between 0.55 and 0.65% by weight and the silicon content of the steel is between 0.08 and 0.12% by weight.

### Claim 6 (depends on 1, 2, 3, 4)

The process as claimed in any one of claims 1 to 4, characterized in that, in addition, the manganese content of the steel is between 0.95 and 1.05% by weight and the silicon content of the steel is between 0.16 and 0.20% by weight.

### Claim 7 (depends on 1, 2, 3, 4, 5, 6)

The process as claimed in any one of claims 1 to 6, characterized in that, in addition, the nitrogen content of the steel is less than 0.005% by weight.

### Claim 8 (depends on 1, 2, 3, 4, 5, 6, 7)

The process as claimed in any one of claims 1 to 7, characterized in that, in addition, the phosphorus content of the steel is less than 0.015% by weight.

### Claim 9 (depends on 1, 2, 3, 4, 5, 6, 7, 8)

A bake hardening sheet that can be obtained by the process as claimed in any one of claims 1 to 8, characterized in that it has a yield strength of between 260 and 360 MPa, a tensile strength of between 320 and 460 MPa, a BH2 value of greater than 40 MPa and a yield plateau of less than or equal to 0.2%.

### Claim 10 (depends on 9)

The sheet as claimed in claim 9, characterized in that it has, in addition, a BH2 value of greater than 60 MPa.

### Claim 11 (depends on 9, 10)