# US 2005/0029115 A1 · Method for producing hard surface, colored, anodized aluminum parts

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2005/0029115 A1
- Document ID: US20050029115A1
- Status: Published application
- Kind: A1
- Application number: 10/635,210
- Filed: 2003-08-06
- Published: 2005-02-10
- Earliest claimed: 2003-08-06
- Assignees: General Motors Corporation
- Inventors: Hong-Hsiang Kuo; Yar-Ming Wang; Joseph Simmer; Hsai-Yin Lee
- Web page: https://patentgrep.com/patent/US20050029115A1

## CPC

- C25D 11/12: Anodising more than once, e.g. in different baths
- C25D 11/22: for colouring layers
- C25D: PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR

## Abstract

The present invention uses a two-step anodizing process to produce a colored anodized coating on the surface of an aluminum part. In accordance with this invention, a thin hard anodized coating layer is first formed on the surface of the aluminum part and then growing a softer a clear anodized coating layer on the surface of the aluminum part underneath the hard coat layer. The soft coat is essentially colorless and suitable for color finishing. This invention drastically improves the wear resistance of the aluminum part while maintaining a desired amount of clarity for effective electrolytic coloring.

## Claims

### Claim 1

A method of making a colored anodized aluminum article with a hard anodized surface, said method comprising:
forming a hard anodized layer on a surface of said aluminum article, said anodized layer having pores and a thickness in the range of about 4 to 10 microns;
forming a clear anodized layer on the surface of said article under said hard anodized layer, said clear anodized layer having pores larger than the pores of said hard anodized layer and said clear anodized layer having a thickness of 7 microns or greater; and
depositing colored particles into the pores of said clear anodized coating to color said aluminum article.

### Claim 2 (depends on 1)

The method as recited in claim 1 where the thickness of said hard layer is 4 to 6 microns and the thickness of said clear layer is 10 to 15 microns.

### Claim 3 (depends on 1)

The method of making a colored anodized aluminum article with a hard anodized surface layer as recited in claim 1 comprising forming said hard layer by anodizing said aluminum article in a first aqueous sulfuric acid bath at a bath temperature below 5° C.

### Claim 4 (depends on 1)

The method of making a colored anodized aluminum article with a hard anodized surface as recited in claim 1 comprising forming said clear layer by anodizing said aluminum article in a second aqueous sulfuric acid bath at a bath temperature above 15° C.

### Claim 5

A method of making a colored anodized aluminum article with a hard anodized surface, said method comprising:
forming a hard anodized layer on a surface of said aluminum article by anodizing said surface in a first sulfuric acid bath using a direct current through said first bath and a bath temperature below 5° C., the thickness of said hard anodized layer being in the range of about 4 to 10 microns;
forming a clear anodized layer on the surface of said aluminum article by anodizing said surface in a second sulfuric acid bath using a direct current through said bath and a bath temperature of above 15° C., the thickness of said clear coating being above 7 microns; and
coloring said aluminum article by depositing colored particles into the pores of said clear anodized coating.

### Claim 6 (depends on 1)

The method as recited in claim 1 comprising immersing said aluminum article with its said porous hard anodized layer and said porous clear anodized layer in an aqueous acid bath comprising a salt of one or more metals and electrolytically depositing particles of said metal from said bath into the pores of said clear anodized layer.

### Claim 7 (depends on 6)

The method as recited in claim 6 comprising electrolytically coloring the aluminum part using a tin sulfate solution.

### Claim 8 (depends on 5)

The method as recited in claim 5 comprising immersing said aluminum article with its said porous hard anodized layer and said porous clear anodized layer in an aqueous acid bath comprising a salt of one or more metals and electrolytically depositing particles of said metal from said bath into the pores of said clear anodized layer.

### Claim 9 (depends on 8)

The method as recited in claim 8 comprising electrolytically coloring the aluminum part using a tin sulfate solution.

### Claim 10

A colored aluminum or aluminum alloy article comprising a surface with a clear porous anodized layer and a hard porous anodized layer overlying said clear layer, the pores of said clear anodized layer containing coloring particles.

### Claim 11 (depends on 10)

The aluminum alloy part as recited in claim 10 wherein said hard anodized layer has a thickness in the range of 4 to 10 microns.

### Claim 12 (depends on 16)

The aluminum alloy part as recited in claim 16 wherein said soft anodized layer has a thickness greater than 10 microns.

### Claim 13 (depends on 10)

The aluminum alloy part as recited in claim 10 wherein said pores of said soft anodized layer each have a diameter of about 9 to 20 nm.

### Claim 14 (depends on 10)

The aluminum alloy part as recited in claim 10 wherein said pores of said hard anodized layer each have a diameter of about 1-2 nm.

### Claim 15 (depends on 10)

The aluminum alloy part as recited in claim 10 wherein said hard anodized layer is formed on a surface of said aluminum article by anodizing said surface in a first sulfuric acid bath using a direct current through said first bath and a bath temperature below 5° C.

### Claim 16 (depends on 10)

The aluminum alloy part as recited in claim 10 wherein said soft, clear anodized layer is formed on the surface of said aluminum article by anodizing said surface in a second sulfuric acid bath using a direct current through said bath and a bath temperature of above 15° C.