- Earliest claimed: 2002-12-20
- Assignees: Conoco Inc.
- Inventors: Rafael L. Espinoza; Kandaswamy Jothimurugesan
- Web page: https://patentgrep.com/patent/US20040122115A1

## CPC

- B01J 23/8946: {with alkali or alkaline earth metals}
- B01J 23/8953: {with zinc, cadmium or mercury}
- B01J 23/8986: {with manganese, technetium or rhenium}
- B01J 37/031: {Precipitation}
- B01J: CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS

## Abstract

The present invention presents an iron-based Fischer-Tropsch catalyst having a low water-gas shift activity and high selectivity and productivity toward a hydrocarbon wax wherein said catalyst comprises iron; silver; sodium, lithium, potassium, rubidium and/or cesium; optionally, calcium, magnesium, boron, and/or aluminum; and a silica structural promoter. The present invention further presents a method of making a precipitated iron-based Fischer-Tropsch catalyst. The present invention still further presents a process for producing hydrocarbons using the iron-based, precipitated Fischer-Tropsch catalyst of the present invention.

## Claims

### Claim 1

A Fischer-Tropsch catalyst comprising
iron;
silver;
optionally, at least one selected from the group consisting of manganese, zinc and the combination thereof;
at least one first promoter selected from the group consisting of sodium, lithium, potassium, rubidium, cesium and any combination thereof;
optionally, at least one second promoter selected from the group consisting of calcium, magnesium, boron, aluminum and any combination thereof; and
at least one structural promoter.

### Claim 2 (depends on 1)

The catalyst of claim 1 wherein the catalyst is capable of producing a product mixture comprising a hydrocarbon wax when contacted with a reactant gas mixture comprising carbon monoxide and hydrogen under suitable conditions of temperature and pressure.

### Claim 3 (depends on 1)

The catalyst of claim 1 wherein the iron is present in an amount between 50 wt % and 95 wt % of metal to total weight of catalyst.

### Claim 4 (depends on 1)

The catalyst of claim 1 wherein the iron is present in an amount between 60 wt % and 90 wt % of metal to total weight of catalyst.

### Claim 5 (depends on 1)

The catalyst of claim 1 wherein the iron is present in an amount between 70 wt % and 90 wt % of metal to total weight of catalyst.

### Claim 6 (depends on 1)

The catalyst of claim 1 wherein the silver is present in an amount between 0.001 wt % and 5 wt % of metal to total weight of catalyst.

### Claim 7 (depends on 1)

The catalyst of claim 1 wherein the silver is present in an amount between 0.001 wt % and 2 wt % of metal to total weight of catalyst.

### Claim 8 (depends on 1)

The catalyst of claim 1 wherein the silver is present in an amount between 0.005 wt % and 1 wt % of metal to total weight of catalyst.

### Claim 9 (depends on 1)

The catalyst of claim 1 wherein one first promoter is lithium.

### Claim 10 (depends on 9)

The catalyst of claim 9 wherein lithium is present in an amount between about 0.05 wt % and about 5 wt % of metal to total weight of catalyst.

### Claim 11 (depends on 9)

The catalyst of claim 9 wherein lithium is present in an amount between about 0.5 wt % and about 2 wt %.

### Claim 12 (depends on 9)

The catalyst according to claim 9 wherein one second promoter is calcium.

### Claim 13 (depends on 12)

The catalyst according to claim 12 characterized by a C5+ productivity of at least about 80 g C5+/h/kg catalyst.

### Claim 14 (depends on 12)

The catalyst according to claim 12 wherein the catalyst is characterized by
an Anderson-Schulz-Flory α value of at least about 0.84.

### Claim 15 (depends on 1)

The catalyst of claim 1 comprising at least two first promoters.

### Claim 16 (depends on 15)

The catalyst of claim 15 wherein two first promoters are potassium and lithium.

### Claim 17 (depends on 16)

The catalyst of claim 16 wherein lithium is present in an amount between about 0.05 wt % and about 5 wt % of metal to total weight of catalyst.

### Claim 18 (depends on 16)

The catalyst of claim 16 wherein lithium is present in an amount between about 0.5 wt % and about 2 wt % of metal to total weight of catalyst.

### Claim 19 (depends on 16)

The catalyst of claim 16 wherein potassium is present in an amount between about 0.0001 wt % and about 1 wt % of metal to total weight of catalyst.

### Claim 20 (depends on 16)

The catalyst of claim 16 wherein potassium is present in an amount between about 0.0005 wt % and about 0.5 wt % of metal to total weight of catalyst.

### Claim 21 (depends on 16)

The catalyst of claim 16 wherein potassium is present in an amount between about 0.0005 wt % and about 0.1 wt % of metal to total weight of catalyst.

### Claim 22 (depends on 1)

The catalyst of claim 1 wherein the first promoter is present in an amount between about 0.0005 wt % and about 0.05 wt % of metal to total weight of support.

### Claim 23 (depends on 1)

The catalyst according to claim 1 wherein said second promoters comprise calcium, magnesium or the combination thereof.

### Claim 24 (depends on 23)

The catalyst of claim 23 wherein at least one second promoter is calcium.

### Claim 25 (depends on 24)

The catalyst of claim 24 wherein calcium is present in an amount between about 0.001 wt % and about 4 wt % of element to total weight of catalyst.

### Claim 26 (depends on 24)

The catalyst of claim 24 wherein calcium is present in an amount between 0.5 wt % and 3 wt % of element to total weight of catalyst.

### Claim 27 (depends on 1)

The catalyst according to claim 1 wherein the structural promoter comprising at least one metal oxide is selected from the group consisting of silica, alumina, zirconia, titania, or any combination thereof.

### Claim 28 (depends on 27)

The catalyst according to claim 27 wherein the catalyst is characterized by
a physical catalyst attrition of less than about 8%.

### Claim 29 (depends on 28)

The catalyst according to claim 28 wherein the catalyst is used in a slurry bubble column reactor or a fixed bed reactor.

### Claim 30 (depends on 27)

The catalyst according to claim 27 wherein the catalyst is characterized by
a physical catalyst attrition of less than about 6%.

### Claim 31 (depends on 1)

The catalyst according to claim 1 wherein a structural promoter comprises between about 5 and about 45 parts by weight (pbw) of a metal oxide per 100 parts iron.

### Claim 32 (depends on 31)

The catalyst according to claim 31 wherein the metal oxide comprises at least one selected from the group consisting of silica, alumina, or the combination thereof.

### Claim 33 (depends on 31)

The catalyst according to claim 31 wherein the metal oxide comprises silica.

### Claim 34 (depends on 33)

The catalyst according to claim 33 wherein the silica comprises between about 50% and about 80% silica from a colloidal silica.

### Claim 35 (depends on 34)

The catalyst according to claim 34 wherein the colloidal silica has an average particle size between about 10 nm and about 100 nm.

### Claim 36 (depends on 33)

The catalyst according to claim 33 wherein the silica comprises between about 20% and about 50% silica from silicic acid.

### Claim 37 (depends on 33)

The catalyst according to claim 33 wherein silica comprises between about 15 and about 35 parts by weight (pbw) silica per 100 parts iron.

### Claim 38 (depends on 37)

The catalyst according to claim 37 wherein the silica comprises between about 50% and about 80% silica from colloidal silica and between about 20% and about 50% silica from silicic acid.

### Claim 39 (depends on 1)

The catalyst according to claim 1 wherein the catalyst is characterized by
a CO2 selectivity not greater than about 18 mol % CO2.

### Claim 40 (depends on 1)

The catalyst according to claim 1 wherein the catalyst is characterized by
a CO2 selectivity not greater than about 13 mol % CO2.

### Claim 41 (depends on 1)

The catalyst according to claim 1 wherein the catalyst is characterized by
a physical catalyst attrition of less than about 8%.

### Claim 42 (depends on 41)

The catalyst according to claim 41 wherein the catalyst is characterized by
a physical catalyst attrition of less than about 6%.

### Claim 43 (depends on 1)

The catalyst according to claim 1 wherein the catalyst is characterized by
a CH4 selectivity not greater than about 6 wt % CH4.

### Claim 44 (depends on 1)

The catalyst according to claim 1 wherein the catalyst is characterized by
an Anderson-Schulz-Flory a value of at least about 0.84.

### Claim 45 (depends on 1)

The catalyst according to claim 1 wherein the catalyst is used in a slurry bubble column reactor or a fixed bed reactor.

### Claim 46

A method of making a Fischer-Tropsch catalyst comprising
the steps of precipitating
at least one iron compound;
optionally, at least one silver compound;
optionally, at least one manganese compound; and
optionally, at least one zinc compound;
from a suitable solution and under suitable conditions to provide a precipitate;
optionally, washing the precipitate to provide a clean precipitate;
adding at least one first promoter compound to a slurry comprising the clean precipitate;
optionally, adding at least one second promoter compound to a slurry comprising the clean precipitate;
adding at least one structural promoter compound to a slurry comprising the clean precipitate to provide a precursor slurry;
spray-drying the precursor slurry to provide catalyst precursor particles;
calcining the catalyst precursor particles under suitable conditions to provide a calcined precatalyst;
optionally, impregnating the calcined precatalyst with a compound comprising at least one selected from the group consisting of silver, sodium, lithium, potassium, rubidium, cesium and any combination thereof to provide the catalyst;
drying the catalyst under suitable conditions to provide a dry catalyst;
calcining the dry catalyst under suitable conditions to provide the catalyst; and
optionally, reducing the catalyst under conditions suitable for providing the reduced catalyst.

### Claim 47 (depends on 46)

The method according to claim 46 comprising
precipitating at least one iron compound from a suitable solution and under suitable conditions to provide a precipitate;
washing the precipitate to provide a clean precipitate;
adding
at least two first promoter compounds including a compound comprising lithium and a compound comprising potassium,
at least one second promoter compound including a compound comprising calcium, and
at least one structural promoter compound comprising a metal oxide sol
to a slurry comprising the clean precipitate to provide a precursor slurry;
spray-drying the precursor slurry to provide catalyst precursor particles;
calcining the catalyst precursor particles under suitable conditions to provide a calcined precatalyst;
impregnating the calcined precatalyst with a compound comprising silver to provide the catalyst;
drying the catalyst under suitable conditions to provide a dry catalyst; and
calcining the dry catalyst under suitable conditions.

### Claim 48 (depends on 46)

The method according to claim 46 comprising
precipitating
at least one iron compound,
at least one silver compound;
optionally at least one manganese compound; and
optionally, at least one zinc compound;
from a suitable solution to provide a precipitate,
optionally, washing the co-precipitate to provide a clean precipitate;
adding
at least one first promoter compound and
at least one second promoter compound
at least one structural promoter compound comprising a metal oxide to a slurry comprising the clean precipitate to provide a precursor slurry;
spray-drying the precursor slurry to provide catalyst precursor particles;
calcining the catalyst precursor particles under suitable conditions to provide a calcined precatalyst;
impregnating the calcined precatalyst with another first promoter compound to provide the catalyst;
drying the catalyst under suitable conditions to provide a dry catalyst; and
calcining the dry catalyst under suitable conditions.

### Claim 49 (depends on 46)

The method according to claim 46 comprising
precipitating
at least one iron compound,
at least one silver compound,
optionally, at least one manganese compound, and
optionally, at least one zinc compound
from a suitable solution and under suitable conditions to provide a precipitate;
optionally, washing the precipitate to provide a clean precipitate;
adding
at least one first promoter compound comprising lithium;
at least one second promoter compound comprising calcium
at least one structural promoter compound comprising a metal oxide sol to a slurry comprising the clean precipitate to provide a precursor slurry;
spray-drying the precursor slurry to provide catalyst precursor particles;
calcining the catalyst precursor particles under suitable conditions to provide a calcined precatalyst;
impregnating the calcined precatalyst with a compound comprising potassium to provide the catalyst;
drying the catalyst under suitable conditions to provide a dry catalyst; and
calcining the dry catalyst under suitable conditions.

### Claim 50 (depends on 46)

The method according to claim 46 wherein any one step of precipitating is carried out more than once.

### Claim 51 (depends on 46)

The method according to claim 46 wherein any two or more steps of precipitating are carried out sequentially.

### Claim 52 (depends on 46)

The method according to claim 46 wherein any two or more steps of precipitating are carried out simultaneously.

### Claim 53 (depends on 46)

The method according to claim 46 wherein the precipitate comprises at least one selected from the group consisting of iron oxides, iron hydroxides, and iron oxyhydroxides.

### Claim 54 (depends on 46)

The method according to claim 46 wherein the suitable solution comprises at least one or any combination of soluble iron compounds selected from the group consisting of iron halides, iron nitrates, iron chlorides and iron acetates.

### Claim 55 (depends on 54)

The method according to claim 54 wherein the soluble iron compound is iron nitrate nonahydrate.

### Claim 56 (depends on 46)

The method according to claim 46 wherein precipitating at least one iron compound from a suitable solution and under suitable conditions to provide a precipitate comprises adding a sufficient quantity of a basic solution.

### Claim 57 (depends on 56)

The method according to claim 56 wherein the basic solution comprises one selected from the group consisting of ammonium carbonate, ammonium bicarbonate, ammonium hydroxide, sodium carbonate and sodium bicarbonate.

### Claim 58 (depends on 56)

The method according to claim 56 wherein the concentration of the basic solution is between about 1M and 3M.

### Claim 59 (depends on 56)

The method according to claim 56 wherein a suitable solution comprises a soluble iron compound.

### Claim 60 (depends on 59)

The method according to claim 59 wherein a soluble iron compound is iron(III) nitrate nonahydrate.

### Claim 61 (depends on 56)

The method according to claim 56 wherein suitable conditions comprise a pH between about 6 and about 9.

### Claim 62 (depends on 46)

The method according to claim 46 wherein the precipitate is washed with deionized water under vacuum filtration.

### Claim 63 (depends on 46)

The method according to claim 46 wherein at least two first promoter compounds are added to a slurry comprising the clean precipitate.

### Claim 64 (depends on 63)

The method according to claim 63 wherein two first promoter compounds comprise lithium and potassium.

### Claim 65 (depends on 46)

The method according to claim 46 wherein at least one first promoter compound comprises lithium.

### Claim 66 (depends on 65)

The method according to claim 65 wherein a compound of lithium is selected from the group consisting of lithium nitrate (LiNO3) and lithium carbonate (Li2CO3).

### Claim 67 (depends on 46)

The method according to claim 46 wherein at least one structural promoter compound is added concurrently, simultaneously or sequentially with respect to at least one first promoter compound.

### Claim 68 (depends on 67)

The method according to claim 67 wherein a first promoter compound comprises lithium and a structural promoter compound comprises silicic acid.

### Claim 69 (depends on 46)

The method according to claim 46 wherein a structural promoter is selected from the group consisting of silica, alumina, zirconia, titania and any combination thereof.

### Claim 70 (depends on 46)

The method according to claim 46 wherein a structural promoter comprises between about 5 and about 45 parts by weight (pbw) of a metal oxide per 100 parts iron.

### Claim 71 (depends on 70)

The method according to claim 70 wherein the structural promoter comprises at least one selected from the group consisting of silica, alumina and any combination thereof.

### Claim 72 (depends on 71)

The method according to claim 71 wherein the structural promoter comprises silica.

### Claim 73 (depends on 72)

The method according to claim 72 wherein the silica comprises between about 50% and about 80% silica from a colloidal silica.

### Claim 74 (depends on 73)

The method according to claim 73 wherein the colloidal silica has an average particle size between about 10 nm and about 100 mm.

### Claim 75 (depends on 72)

The method according to claim 72 wherein the silica comprises between about 20% and about 50% silica from silicic acid.

### Claim 76 (depends on 72)

The method according to claim 72 wherein silica comprises between about 15 and about 35 parts by weight (pbw) silica per 100 parts iron.

### Claim 77 (depends on 76)

The method according to claim 76 wherein the silica comprises between about 50% and about 80% silica from colloidal silica and between about 20% and about 50% silica from silicic acid.

### Claim 78 (depends on 46)

The method according to claim 46 wherein at least two structural promoter compounds are added.

### Claim 79 (depends on 78)

The method according to claim 78 wherein two structural promoter compounds comprise silicic acid and colloidal silica, respectively.

### Claim 80 (depends on 79)

The method according to claim 79 wherein the colloidal silica has an average particle size between about 10 nm and about 100 nm.

### Claim 81 (depends on 79)

The method according to claim 79 wherein the colloidal silica is AS-40 colloidal silica from Aldrich having an average particle size of about 22 nm.

### Claim 82 (depends on 79)

The method according to claim 79 wherein silicic acid and colloidal silica are added in amounts effective for providing in the spray-dried product a total silica content of between about 5 parts of silica and about 45 parts of silica per 100 parts iron.

### Claim 83 (depends on 82)

The method according to claim 82 wherein silicic acid is added in an amount effective for providing in the spray-dried product between about 20% and about 50% of silica from silicic acid.

### Claim 84 (depends on 79)

The method according to claim 79 wherein silicic acid and colloidal silica are added in amounts effective for providing in the spray-dried product a total of between about 15 and about 35 parts of silica per 100 parts iron.

### Claim 85 (depends on 84)

The method according to claim 84 wherein silicic acid and colloidal silica are added in amounts effective for providing in the spray-dried product between about 20 and about 50% of parts by weight of silica is from colloidal silica and between about 50% and 80% of parts by weight of silica from silicic acid.

### Claim 86 (depends on 46)

The method according to claim 46 wherein said first and second promoter compounds may be added in any order or simultaneously.

### Claim 87 (depends on 86)

The method according to claim 86 wherein said first promoter compound comprises lithium and said second promoter compound comprises calcium.

### Claim 88 (depends on 46)

The method according to claim 46 wherein suitable conditions for calcining the catalyst particles comprise a temperature between about 200° C. and about 500° C.

### Claim 89 (depends on 46)

The method according to claim 46 wherein suitable conditions for calcining the catalyst particles comprise a temperature between about 250° C. and about 400° C.

### Claim 90 (depends on 46)

The method according to claim 46 wherein suitable conditions for calcining the catalyst particles comprise calcining for a period of time between about 0.5 hours and about 24 hours.

### Claim 91 (depends on 46)

The method according to claim 46 wherein suitable conditions for calcining the catalyst particles comprise calcining for a period of time between about 1 hour and about 5 hours.

### Claim 92 (depends on 46)

The method according to claim 46 wherein the calcined precatalyst is impregnated with a compound comprising silver.

### Claim 93 (depends on 92)

The method according to claim 92 wherein silver(I) nitrate is the compound comprising silver.

### Claim 94 (depends on 46)

The method according to claim 46 wherein impregnating the calcined precatalyst is carried out using a technique of incipient wetness impregnation.

### Claim 95 (depends on 46)

The method according to claim 46 wherein suitable conditions for drying the catalyst comprise a temperature between about 80° C. and about 150° C.; and an interval of time between about 2 hours and about 20 hours.

### Claim 96 (depends on 46)

The method according to claim 46 wherein suitable conditions for calcining the dry catalyst comprise a temperature between about 200° C. and about 350° C.

### Claim 97 (depends on 46)

The method according to claim 46 wherein suitable conditions for calcining the dry catalyst comprise a temperature between about 250° C. and 300° C.

### Claim 98 (depends on 46)

The method according to claim 46 wherein suitable conditions for calcining the dry catalyst comprise calcining for a period of time between about 0.5 hours and about 10 hours.

### Claim 99 (depends on 46)

The method according to claim 46 wherein suitable conditions for calcining the dry catalyst comprise calcining for a period of time between about 1 hour and about 5 hours.

### Claim 100 (depends on 46)

The method according to claim 46 wherein suitable conditions for reducing the catalyst comprise exposure to a suitable gas at elevated temperature.

### Claim 101 (depends on 100)

The method according to claim 100 wherein a suitable gas comprises at least one selected from the group consisting of hydrogen, carbon monoxide and the combination thereof.

### Claim 102 (depends on 101)

The method according to claim 101 wherein a suitable gas comprises between 1% and 100% hydrogen by volume.

### Claim 103 (depends on 101)

The method according to claim 101 wherein a suitable gas comprises between about 1% and about 100% carbon monoxide by volume.

### Claim 104 (depends on 100)

The method according to claim 100 wherein suitable conditions comprise exposing the catalyst to a suitable gas at a temperature between about 75° C. and about 500° C.; for a period of time between about 0.5 hours and about 50 hours; and a pressure between about 1 atm and about 75 atm.

### Claim 105 (depends on 46)

The method according to claim 46 wherein the catalyst is characterized by
a CO2 selectivity not greater than about 18 mol % CO2.

### Claim 106 (depends on 46)

The method according to claim 46 wherein the catalyst is characterized by
a CO2 selectivity not greater than about 13 mol % CO2.

### Claim 107 (depends on 46)

The method according to claim 46 wherein the catalyst is characterized by
a physical catalyst attrition of less than about 8%.

### Claim 108 (depends on 46)

The method according to claim 46 wherein the catalyst is characterized by
a physical catalyst attrition of less than about 6%.

### Claim 109 (depends on 46)

The catalyst made according to the method according to claim 46.

### Claim 110

A process for producing hydrocarbons comprising
contacting a reactant gas mixture comprising synthesis gas with a Fischer-Tropsch catalyst comprising
iron;
silver;
optionally, at least one selected from the group consisting of manganese, zinc and the combination thereof;
at least one first promoter selected from the group consisting of sodium, lithium, potassium, rubidium, cesium and any combination thereof;
optionally, at least one second promoter selected from the group consisting of calcium, magnesium, boron, aluminum and any combination thereof; and
at least one structural promoter;
under suitable conditions and in a suitable reactor.

### Claim 111 (depends on 110)

The process according to claim 110 wherein the process is effective for producing a product mixture comprising hydrocarbon wax.

### Claim 112 (depends on 110)

The process according to claim 110 wherein the ratio of H2:CO in said synthesis gas is between about 1:1 and about 4:1.

### Claim 113 (depends on 110)

The process according to claim 110 wherein the ratio of H2:CO in said synthesis gas is between about 1.4:1 and about 2.3:1.

### Claim 114 (depends on 110)

The process according to claim 110 wherein the Fischer-Tropsch catalyst comprises iron, silver, a lithium first promoter, a calcium second promoter and two structural promoters comprising a metal oxide.

### Claim 115 (depends on 110)

The process according to claim 110 wherein a structural promoter comprises at least one metal oxide selected from the group consisting of silica, alumina, zirconia, titania and any combination thereof.

### Claim 116 (depends on 110)

The process according to claim 110 wherein a structural promoter comprises a metal oxide which comprises between about 5 and about 45 parts by weight (pbw) of a metal oxide per 100 parts iron.

### Claim 117 (depends on 116)

The process according to claim 116 wherein the structural promoter comprises at least one selected from the group consisting of silica, alumina and the combination thereof.

### Claim 118 (depends on 117)

The process according to claim 117 wherein the structural promoter comprises silica.

### Claim 119 (depends on 118)

The process according to claim 118 wherein the silica comprises between about 50% and about 80% silica from a colloidal silica.

### Claim 120 (depends on 119)

The process according to claim 119 wherein the colloidal silica has an average particle size between about 10=m and about 100 nm.

### Claim 121 (depends on 118)

The process according to claim 118 wherein the silica comprises between about 20% and about 50% silica from silicic acid.

### Claim 122 (depends on 118)

The process according to claim 118 wherein silica comprises between about 15 and about 35 parts by weight (pbw) silica per 100 parts iron.

### Claim 123 (depends on 122)

The process according to claim 122 wherein the silica comprises between about 50% and about 80% silica from colloidal silica and between about 20% and about 50% silica from silicic acid.

### Claim 124 (depends on 114)

The process according to claim 114 wherein two structural promoters are silicic acid and colloidal silica.

### Claim 125 (depends on 114)

The process according to claim 114 wherein two structural promoters comprising silicon comprise between about 5 and about 45 parts by weight (pbw) silica per 100 parts iron.

### Claim 126 (depends on 125)

The process according to claim 125 wherein the silica comprises between about 20% and about 50% silica from silicic acid.

### Claim 127 (depends on 110)

The process according to claim 110 wherein said hydrocarbon wax comprises C18+ hydrocarbons.

### Claim 128 (depends on 110)

The process according to claim 110 wherein said product mixture is characterized by an α of at least 0.84.

### Claim 129 (depends on 110)

The process according to claim 110 wherein C5+ hydrocarbons are produced at a rate of at least 50 g C5+/h/kg cat.

### Claim 130 (depends on 129)

The process according to claim 129 wherein C5+ hydrocarbons are produced at a rate of at least 80 g C5+/h/kg cat.

### Claim 131 (depends on 110)

The process according to claim 110 wherein methane comprises not more than about 6 wt % of said product mixture.

### Claim 132 (depends on 110)

The process according to claim 110 wherein the catalyst is characterized by
a CO2 selectivity not greater than about 18 mol % CO2.

### Claim 133 (depends on 110)

The process according to claim 110 wherein the catalyst is characterized by
a CO2 selectivity not greater than about 13 mol % CO2.

### Claim 134 (depends on 110)

The process according to claim 110 wherein the catalyst is characterized by
a physical catalyst attrition of less than about 8%.

### Claim 135 (depends on 110)

The process according to claim 110 wherein the catalyst is characterized by
a physical catalyst attrition of less than about 6%.

### Claim 136 (depends on 110)

The process according to claim 110 wherein a suitable reactor is selected from the group consisting of fixed bed, ebulliating bed, fluidized bed, entrained bed and slurry bubble column reactors.

### Claim 137 (depends on 136)

The process according to claim 136 wherein a suitable reactor is selected from the group consisting of slurry bubble column and fixed bed reactors.

### Claim 138 (depends on 110)

The process according to claim 110 wherein suitable conditions comprise a temperature between about 180° C. and about 300° C. and a pressure between about 80 psia (552 kPa) and about 1000 psia (6895 kPa).