# US 2004/0079927 A1 · ESD dissipative ceramics

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2004/0079927 A1
- Document ID: US20040079927A1
- Status: Published application
- Kind: A1
- Application number: 10/689,192
- Filed: 2003-10-20
- Published: 2004-04-29
- Earliest claimed: 2000-11-21
- Assignees: Saint-Gobain Ceramics & Plastics, Inc.
- Inventors: Oh-Hun Kwon; Matthew A. Simpson; Roger J. Lin
- Web page: https://patentgrep.com/patent/US20040079927A1

## CPC

- C04B 35/486: Fine ceramics
- C04B 33/14: Colouring matters
- C04B 33/20: for dry-pressing (C04B33/13 takes precedence)
- C04B 33/32: Burning methods
- C04B 35/453: based on zinc, tin, or bismuth oxides or solid solutions thereof with other oxides, e.g. zincates, stannates or bismuthates
- C04B 35/457: based on tin oxides or stannates
- C04B 35/488: Composites
- C04B 35/4885: {with aluminium oxide}
- C04B 35/581: based on aluminium nitride
- C04B 35/64: Burning or sintering processes (C04B33/32 takes precedence {; powder metallurgy B22F})
- C04B 35/6455: {Hot isostatic pressing}
- C04B 2235/3215: Barium oxides or oxide-forming salts thereof
- C04B 2235/3217: Aluminum oxide or oxide forming salts thereof, e.g. bauxite, alpha-alumina
- C04B 2235/3224: Rare earth oxide or oxide forming salts thereof, e.g. scandium oxide
- C04B 2235/3225: Yttrium oxide or oxide-forming salts thereof
- C04B 2235/3227: Lanthanum oxide or oxide-forming salts thereof
- C04B 2235/3241: Chromium oxides, chromates, or oxide-forming salts thereof
- C04B 2235/3243: Chromates or chromites, e.g. aluminum chromate, lanthanum strontium chromite
- C04B 2235/3246: Stabilised zirconias, e.g. YSZ or cerium stabilised zirconia
- C04B 2235/3248: Zirconates or hafnates, e.g. zircon
- C04B 2235/3265: Mn2O3
- C04B 2235/3268: Manganates, manganites, rhenates or rhenites, e.g. lithium manganite, barium manganate, rhenium oxide
- C04B 2235/3272: Iron oxides or oxide forming salts thereof, e.g. hematite, magnetite
- C04B 2235/3274: Ferrites
- C04B 2235/3281: Copper oxides, cuprates or oxide-forming salts thereof, e.g. CuO or Cu2O
- C04B 2235/3284: Zinc oxides, zincates, cadmium oxides, cadmiates, mercury oxides, mercurates or oxide forming salts thereof
- C04B 2235/3293: Tin oxides, stannates or oxide forming salts thereof, e.g. indium tin oxide [ITO]
- C04B 2235/3294: Antimony oxides, antimonates, antimonites or oxide forming salts thereof, indium antimonate
- C04B 2235/3826: Silicon carbides
- C04B 2235/3839: Refractory metal carbides
- C04B 2235/5409: expressed by specific surface values
- C04B 2235/604: Pressing at temperatures other than sintering temperatures
- C04B 2235/656: characterised by specific heating conditions during heat treatment
- C04B 2235/6562: Heating rate
- C04B 2235/6567: Treatment time
- C04B 2235/6582: Hydrogen containing atmosphere
- C04B 2235/661: Multi-step sintering
- C04B 2235/663: Oxidative annealing
- C04B 2235/664: Reductive annealing
- C04B 2235/765: Tetragonal symmetry
- C04B 2235/767: Hexagonal symmetry, e.g. beta-Si3N4, beta-Sialon, alpha-SiC or hexa-ferrites
- C04B 2235/77: Density
- C04B 2235/785: Submicron sized grains, i.e. from 0,1 to 1 micron
- C04B 2235/786: Micrometer sized grains, i.e. from 1 to 100 micron
- C04B 2235/80: Phases present in the sintered or melt-cast ceramic products other than the main phase
- C04B 2235/96: Properties of ceramic products, e.g. mechanical properties such as strength, toughness, wear resistance
- C04B 2235/963: Surface properties, e.g. surface roughness
- C04B 2235/9661: Colour
- C04B 2235/9669: Resistance against chemicals, e.g. against molten glass or molten salts
- H05K 1/0254: {High voltage adaptations; Electrical insulation details; Overvoltage or electrostatic discharge protection (electrostatic discharge protection for electric apparatus in general H05K9/0067, H05K9/0079); Arrangements for regulating voltages or for using plural voltages}
- H05K 1/0306: {Inorganic insulating substrates, e.g. ceramic, glass}
- C04B: LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE {(roofing granules E04D7/005)}; CERAMICS (devitrified glass-ceramics C03C10/00); REFRACTORIES; TREATMENT OF NATURAL STONE
- H05K: PRINTED CIRCUITS; CASINGS OR CONSTRUCTIONAL DETAILS OF ELECTRIC APPARATUS; MANUFACTURE OF ASSEMBLAGES OF ELECTRICAL COMPONENTS

## Abstract

This invention relates to a dense ceramics having ESD dissipative characteristics, tunable volume and surface resistivities in semi-insulative range (103-1011 Ohm-cm), substantially pore free, high flexural strength, light colors, for desired ESD dissipation characteristics, structural reliability, high vision recognition, low wear and particulate contamination to be used as ESD dissipating tools, fixtures, load bearing elements, work surfaces, containers in manufacturing and assembling electrostatically sensitive microelectronic, electromagnetic, electro-optic components, devices and systems.

## Claims

### Claim 1

An ESD dissipative ceramic composition formed by sintering a mixture comprising a base material and one or more resistivity modifiers for a sufficient time and at a sufficient temperature to achieve at least 99 percent of the theoretical density,
wherein the base material comprises a tetragonal zirconia polycrystal (TZP);
wherein the resistivity modifier comprises from about 5 vol. % to 60 vol. % of the base material and is selected from the group consisting of conductive and semiconductive materials or mixtures thereof;
and wherein the ESD dissipative ceramic composition has the following physical properties:
(a) volume resistivity ranging from 103-1011 Ohm-cm;
(b) flexural strength of at least 500 MPa; and
(c) voltage decay time of less than 500 ms.

### Claim 2 (depends on 1)

The ESD dissipative ceramic composition of claim 1, wherein the TZP comprises yttria stabilized TZP (Y-TZP) wherein the yttria is present at from about 2.5 to 4.5 mole percent.

### Claim 3 (depends on 2)

The ESD dissipative ceramic composition of claim 2, wherein the Y-TZP comprises 2.6 mole percent yttria.

### Claim 4 (depends on 2)

The ESD dissipative ceramic composition of claim 2, wherein the Y-TZP comprises 2.8 mole percent yttria.

### Claim 5 (depends on 2)

The ESD dissipative ceramic composition of claim 2, wherein the Y-TZP comprises 3 mole percent yttria.

### Claim 6 (depends on 1)

The ESD dissipative ceramic composition of claim 1, wherein the resistivity modifier comprises from about 10 vol. % to 50 vol. % of the base material.

### Claim 7 (depends on 1)

The ESD dissipative ceramic composition of claim 1, wherein the resistivity modifier comprises from about 20 vol. % to 40 vol. % of the base material.

### Claim 8 (depends on 1)

The ESD dissipative ceramic composition of claim 1, wherein the resistivity modifier comprises from about 25 vol. % to 30 vol. % of the base material.

### Claim 9 (depends on 1)

The ESD dissipative ceramic composition of claim 1, wherein the resistivity modifiers is selected from the group consisting of oxides, carbides, nitrides, oxycarbides, oxynitrides, and oxycarbonitrides.

### Claim 10 (depends on 1)

The ESD dissipative ceramic composition of claim 1, wherein the flexural strength is at least 600 MPa.

### Claim 11 (depends on 1)

The ESD dissipative ceramic composition of claim 1, wherein the flexural strength is at least 700 MPa.

### Claim 12 (depends on 1)

The ESD dissipative ceramic composition of claim 1, wherein the flexural strength is at least 800 MPa.

### Claim 13 (depends on 1)

The ESD dissipative ceramic composition of claim 1, wherein the flexural strength is at least 900 MPa.

### Claim 14 (depends on 1)

The ESD dissipative ceramic composition of claim 1, wherein the flexural strength is at least 1000 MPa.

### Claim 15 (depends on 1)

An ESD dissipative component part made from a ceramic of claim 1, where the component has less than 600 particles/cm2 in the particle generation test and where the component has an Ra of less than 3000 Å.

### Claim 16 (depends on 15)

The ESD dissipative component part of claim 15, wherein the surface finish is produced by tumbling.

### Claim 17 (depends on 15)

The ESD dissipative component part of claim 15, wherein the color of the ceramic is light.

### Claim 18 (depends on 15)

The ESD dissipative component part of claim 15, wherein the color of the ceramic is dark.

### Claim 19

An ESD dissipative ceramic composition formed by sintering a mixture comprising a base material and one or more resistivity modifiers for a sufficient time and at a sufficient temperature to achieve at least 99.5 percent of the theoretical density;
wherein the base material comprises a tetragonal zirconia polycrystal (TZP);
wherein the resistivity modifier comprises from about 5 vol. % to 60 vol. % of the base material and is selected from the group consisting of conductive and semiconductive materials or mixtures thereof;
and wherein the ESD dissipative ceramic composition has the following physical properties:
(a) volume resistivity ranging from 105-109 Ohm-cm;
(b) flexural strength of at least 500 MPa; and
(c) voltage decay time of less than 500 ms.

### Claim 20 (depends on 19)

The ESD dissipative ceramic composition of claim 19, wherein the TZP comprises yttria stabilized TZP (Y-TZP) wherein the yttria is present at from about 2.5 to 4.5 mole percent.

### Claim 21 (depends on 20)

The ESD dissipative ceramic composition of claim 20, wherein the Y-TZP comprises 2.6 mole percent yttria.

### Claim 22 (depends on 20)

The ESD dissipative ceramic composition of claim 20, wherein the Y-TZP comprises 2.8 mole percent yttria.

### Claim 23 (depends on 20)

The ESD dissipative ceramic composition of claim 20, wherein the Y-TZP comprises 3 mole percent yttria.

### Claim 24 (depends on 19)

The ESD dissipative ceramic composition of claim 19, wherein the resistivity modifier comprises from about 10 vol. % to 50 vol. % of the base material.

### Claim 25 (depends on 19)

The ESD dissipative ceramic composition of claim 19, wherein the resistivity modifier comprises from about 20 vol. % to 40 vol. % of the base material.

### Claim 26 (depends on 19)

The ESD dissipative ceramic composition of claim 19, wherein the resistivity modifier comprises from about 25 vol. % to 30 vol. % of the base material.

### Claim 27 (depends on 19)

The ESD dissipative ceramic composition of claim 19, wherein the resistivity modifiers is selected from the group consisting of oxides, carbides, nitrides, oxycarbides, oxynitrides, and oxycarbonitrides.

### Claim 28 (depends on 19)

The ESD dissipative ceramic composition of claim 19, wherein the flexural strength is at least 600 MPa.

### Claim 29 (depends on 19)

The ESD dissipative ceramic composition of claim 19, wherein the flexural strength is at least 700 MPa.

### Claim 30 (depends on 19)

The ESD dissipative ceramic composition of claim 19, wherein the flexural strength is at least 800 MPa.

### Claim 31 (depends on 19)

The ESD dissipative ceramic composition of claim 19, wherein the flexural strength is at least 900 MPa.

### Claim 32 (depends on 19)

The ESD dissipative ceramic composition of claim 19, wherein the flexural strength is at least 1000 MPa.

### Claim 33 (depends on 19)

An ESD dissipative component part made from a ceramic of claim 19, where the component has less than 600 particles/cm1 in the particle generation test and where the component has an Ra of less than 3000 Å.

### Claim 34 (depends on 33)

The ESD dissipative component part of claim 33, wherein the surface finish is produced by tumbling.

### Claim 35 (depends on 33)

The ESD dissipative component part of claim 33, wherein the color of the ceramic is light.

### Claim 36 (depends on 33)

The ESD dissipative component part of claim 33, wherein the color of the ceramic is dark.

### Claim 37

An ESD dissipative ceramic composition comprising from about 85 to 60 vol. % Y-TZP and from about 15 to 40 vol. % ZnO densified to at least 95% of the theoretical density by sintering as the primary heat treatment.

### Claim 38 (depends on 37)

The ESD dissipative ceramic composition of claim 37, wherein a secondary heat treatment is employed to increase the theoretical density to greater than 99%.

### Claim 39 (depends on 37)

The ESD dissipative ceramic composition of claim 37, wherein the composition has an L* color measurement of at least 50 using the CIE 1976 L*a*b* scale on an XLE colorimeter.

### Claim 40

An ESD dissipative ceramic composition comprising from about 90 to 50 vol. % Y-TZP and from about 10 to 50 vol. % semi-conductive SnO2 densified to at least 95% of the theoretical density by sintering as the primary heat treatment.

### Claim 41 (depends on 40)

The ESD dissipative ceramic composition of claim 40, wherein the composition has an L* color measurement of at least 50 using the CIE 1976 L*a*b* scale on an LKE calorimeter.

### Claim 42

An ESD dissipative ceramic composition comprising from about 80 to 70 vol. % Y-TZP and from about 20 to 30 vol. % LaMnO3 densified to at least 95% of the theoretical density by sintering as the primary heat treatment.

### Claim 43

An ESD dissipative ceramic composition comprising from about 90 to 60 vol. % Y-TZP and from about 10 to 40 vol. % LaCrO3 densified to at least 99% of the theoretical density by sintering as the primary heat treatment, followed by hot isostatic pressing as the secondary heat treatment.

### Claim 44

An ESD dissipative ceramic composition comprising from about 90 to 75 vol. % Y-TZP and from about 10 to 25 vol. % ZrC densified to at least 95% of the theoretical density by sintering as the primary heat treatment, followed by hot isostatic pressing as the secondary heat treatment.

### Claim 45

An ESD dissipative ceramic composition comprising about 75 vol. % Y-TZP and about 25 vol. % BaO 6Fe2O3 densified to at least 95% of the theoretical density by sintering as the primary heat treatment, followed by hot isostatic pressing as the secondary heat treatment.

### Claim 46

An ESD dissipative ceramic composition comprising AIN heat treated in argon at 1900° C. followed by rapid cooling to room temperature at a rate greater than 10° C./minute.

### Claim 47

An ESD dissipative ceramic comprising ZrO2 and semi-conductive SnO2, said ceramic having the following physical characteristics:
(a) predetermined decay time;
(b) hardness greater than 10 GPa Vickers; and
(c) a density of at least 99% of theoretical.

### Claim 48

An ESD dissipative ceramic composition formed by sintering a mixture comprising a base material and one or more resistivity modifiers;
wherein the base material comprises a tetragonal zirconia polycrystal (TZP);
wherein the resistivity modifier comprises from about 5 vol. % to 60 vol. % of the base material and is selected from the group consisting of conductive and semiconductive materials or mixtures thereof;
and wherein the ESD dissipative-ceramic composition has the following physical properties:
(a) volume resistivity ranging from 106-109 Ohm-cm;
(b) flexural strength of at least 400 MPa; and
(c) voltage decay time of less than 500 ms.

### Claim 49 (depends on 48)

The ESD dissipative ceramic of claim 48, wherein the sintering is conducted in air.

### Claim 50 (depends on 49)

The ESD dissipative ceramic of claim 49, wherein a secondary heat treatment step comprises hot isostatic pressing.

### Claim 51

An ESD dissipative ceramic comprising ZrO2 and semi-conductive SnO2, said ceramic having the following physical characteristics:
(a) predetermined decay time;
(b) hardness greater than 10 GPa Vickers; and
(c) an L* color measurement of at least 50 using the CIE 1976 L*a*b* scale on an LKE calorimeter.

### Claim 52 (depends on 51)

The ESD dissipative ceramic of claim 51, wherein the SnO2 is present in the range of 20-80% by vol of the initial reagents.

### Claim 53

A method of processing ESD dissipative ceramics comprising the steps of:
(a) consolidating two or more powders to a final density by one or more heat treatments, and
(b) using a final heat treatment to produce at least a 25% change in the resistivity of the resulting ceramic.

### Claim 54 (depends on 53)

The process of claim 53, wherein the final heat treatment is conducted in air at less than 90% of the sintering temperature.

### Claim 55 (depends on 53)

The process of claim 53, wherein the final heat treatment is conducted in oxygen at a partial pressure less than that of atmospheric oxygen.

### Claim 56 (depends on 53)

The process of claim 53, wherein the final heat treatment increases the resistance of the resulting ceramic.

### Claim 57 (depends on 53)

The process of claim 53, wherein the final heat treatment decreases the resistance of the resulting ceramic.

### Claim 58 (depends on 53)

The process of claim 53, wherein the final heat treatment moves volume resistivity into the range 106-109 ohm-cm.

### Claim 59

A method of forming light colored ESD dissipative ceramics comprising the steps of:
(a) forming a mixture comprising from about 85 to 60 vol. % Y-TZP and from about 15 to 40 vol. % ZnO; and
(b) densifying the mixture to at least 95% of the theoretical density by a primary heat treatment.

### Claim 60 (depends on 59)

The method of claim 59, further comprising employing a secondary heat treatment step to increase the theoretical density to greater than 99%.

### Claim 61

A method of forming light colored ESD dissipative ceramics comprising the steps of:
(a) forming a mixture comprising from about 90 to 50 vol. % Y-TZP and from about 10 to 50 vol. % semi-conductive SnO2; and
(b) densifying the mixture to at least 95% of the theoretical density by a primary heat treatment.

### Claim 62 (depends on 61)

The method of claim 61, further comprising employing a secondary heat treatment step to increase the theoretical density to greater than 99%.

### Claim 63

A method of modifying the resistivity of ESD dissipative ceramics comprising the step of hot isostatic pressing said ceramics under controlled conditions of heat and atmosphere.

### Claim 64

A method of forming ceramic-based components for ESD-dissipative purposes comprising the steps of:
(a) forming an ESD dissipative ceramic composition;
(b) forming the desired surface finish on said ceramic composition; and
(c) forming ceramic-based components either in whole or in part, in which the ceramics produce less than 600 particles/cm2 in the particle generation test for ESD-dissipative purposes.

### Claim 65 (depends on 64)

The method of claim 64, wherein the surface finish is formed by tumbling.

### Claim 66 (depends on 64)

The method of claim 64, wherein the entire component is formed from the ESD dissipative ceramic composition.

### Claim 67 (depends on 64)

The method of claim 64, wherein only a portion of the component is formed from the ESD dissipative ceramic composition.

### Claim 68 (depends on 64)

An ESD dissipative component, formed by the method of claim 64, wherein the component is selected from the group consisting of MR (magnetoresistive) head substrates, transfer tools for magnetic head manufacturing, tools, fixtures, and containers for HGA (head gimbal assembly), HSA (head stack assembly), HDD (hard disk drive) assembly, tools, fixtures, and containers for wafers handling, processing, and cleaning, tools, fixtures, and containers for wire bonding, trimming, cutting, pick-and-place nozzles for IC chip handling, nozzles for adhesive and solder dispensing, wafer handling fixtures, end effectors, vacuum chucks, IC handling and test fixtures, tools, fixtures, and containers for ESD sensitive devices, assembly fixtures for IC's and magnetic heads, tweezers, screw drivers, scissors, blades, parts for robotic fingers, tools, fixtures, and containers for electro-optic coating process, tools, fixtures, and containers for reticles (photo mask).

### Claim 69

A electrical sensing element formed at least in part from a zirconia-base structural ceramic having a strength of at least 400 MPa, said ceramic further comprising at least 10 vol % ZrO2, wherein electrical conductivity of the ceramic is provided by an additive present as a non-zirconia phase.

### Claim 70 (depends on 69)

The sensing element of claim 69, adapted for or service at room temperature.

### Claim 71 (depends on 69, 70)

The sensing element of claim 69 or 70, adapted for measuring temperature, force, or both temperature and force.

### Claim 72 (depends on 69, 70)

The sensing element of claim 69 or 70, where the non-zirconia phase additive comprises ZnO.

### Claim 73 (depends on 69, 70)

The sensing element of claim 69 or 70, where the conductivity of the ceramic is adjusted so that the sensing region(s) is only part of the whole.

### Claim 74 (depends on 69, 70)

The sensing element of claim 69 or 70, where the responses from two or more sensing regions are detected independently.

### Claim 75

A nonmagnetic ESD dissipative ceramic composition formed by sintering a mixture comprising a base-material and one or more nonmagnetic resistivity modifiers;
wherein the base material comprises a tetragonal zirconia polycrystal (TZP);
wherein the resistivity modifier comprises from about 5 vol. % to 60 vol. % of the base material;
and wherein the ESD dissipative ceramic composition has the following physical properties:
(a) volume resistivity ranging from 106-109 Ohm-cm;
(b) flexural strength of at least 400 MPa; and
(c) a residual flux density no greater than about 10 Gauss.

### Claim 76 (depends on 75)

The nonmagnetic ESD dissipative ceramic composition of claim 75, wherein the resistivity modifiers have a molar magnetic susceptibility of less than 10−3 ml/mol.

### Claim 77 (depends on 76)

The nonmagnetic ESD dissipative ceramic composition of claim 76, wherein the resistivity modifiers are selected from the group consisting of ZnO, SnO2, ZrO2, Y2O3, Al2O3, ZrC, SiC, and mixtures thereof.