# US 2004/0079514 A1 · Production of thin steel strip

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2004/0079514 A1
- Document ID: US20040079514A1
- Status: Published application
- Kind: A1
- Application number: 10/689,284
- Filed: 2003-10-20
- Published: 2004-04-29
- Earliest claimed: 2000-09-29
- Inventors: Lazar Strezov; Kannappar Mukunthan; Walter Blejde; Rama Mahapatra
- Web page: https://patentgrep.com/patent/US20040079514A1

## CPC

- B21B 1/463: {in a continuous process, i.e. the cast not being cut before rolling}
- B22D 11/0622: {formed by two casting wheels}
- B22D 11/124: for cooling
- C21D 8/0215: {Rapid solidification; Thin strip casting}
- C21D 8/0226: {Hot rolling}
- B21B 37/76: Cooling control on the run-out table
- B21B 2201/02: Austenitic rolling
- C21D 1/18: Hardening (C21D1/02 takes precedence); Quenching with or without subsequent tempering (quenching devices C21D1/62)
- C21D 8/0263: {following hot rolling}
- B21B: ROLLING OF METAL (auxiliary operations used in connection with metal-working operations covered in B21, see B21C; bending by rolling B21D; manufacture of particular objects, e.g. screws, wheels, rings, barrels, balls, by rolling B21H; pressure welding by means of a rolling mill B23K20/04)
- B22D: CASTING OF METALS; CASTING OF OTHER SUBSTANCES BY THE SAME PROCESSES OR DEVICES (shaping of plastics or substances in a plastic state B29C; metallurgical processing, selection of substances to be added to metal C21, C22)
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)

## Abstract

A cast carbon steel strip is prepared by continuously casting in a twin roll caster and cooling to transform the strip from austenite to ferrite at a temperature range between 400° C. and 850° C. at a cooling rate of not more than about 100° C./sec, such that the strip has a yield strength of greater than 450 MPa. The cast strip before cooling is passed through a hot rolling mill to reduce the thickness of strip by at least 15% and up to 50%.

## Claims

### Claim 1

A cast steel strip prepared by a process comprising the steps of:
supporting a casting pool of molten low carbon steel on a pair of chilled casting rolls forming a nip between them and continuously casting solidified strip of no more than 5 mm in thickness and including austenite grains by rotating the rolls in mutually opposite directions such that the solidified strip moves downwardly from the nip;
passing the strip through a rolling mill in which it is hot rolled to produce a reduction in the strip thickness of at least 15%, and
cooling the strip to transform the austenite to ferrite within a temperature range between 850° C. and 400° C. and at a cooling rate of more than about 100° C./sec.

### Claim 2 (depends on 1)

The cast steel strip of claim 1, wherein the low carbon steel is a silicon/manganese killed steel, and the strip is hot rolled in the temperature range of 900° C. to 1100° C. and then is cooled at a cooling rate in the range of 100° C./sec to 300° C./sec to produce a final strip having a yield strength of at least 450 MPa.

### Claim 3 (depends on 1)

The cast steel strip of claim 1, wherein the low carbon steel is a silicon/manganese killed steel, and the strip is cooled at a cooling rate in the range of 100° C./sec to 300° C./sec to produce a strip with a final yield strength of at least 450 MPa.

### Claim 4 (depends on 3)

The cast steel strip of claim 3, wherein the final yield strength is between 450 MPa and 700 MPa.

### Claim 5 (depends on 1)

The steel strip of claim 1, wherein the cooling rate is in the range of 100° C./sec to 300° C./sec and the strip has a yield strength of at least 450 MPa.

### Claim 6 (depends on 5)

The cast steel strip of claim 5, wherein the yield strength is between 450 MPa and 700 MPa.

### Claim 7 (depends on 1)

The cast steel strip of claim 1, wherein the low carbon steel is a silicon/manganese killed steel having the following composition by weight:
5 Carbon 0.02-0.08% Manganese 0.30-0.80% Silicon 0.10-0.40% Sulfur 0.002-0.05% Aluminum less than 0.01%

### Claim 8 (depends on 1)

The cast steel strip of claim 1, wherein the low carbon steel is aluminum killed steel.

### Claim 9 (depends on 1)

The cast steel strip of claim 1, wherein the aluminum killed steel has the following composition by weight:
6 Carbon 0.02-0.08% Manganese 0.40% max Silicon 0.05% max Sulfur 0.002-0.05% Aluminum 0.05% max

### Claim 10 (depends on 1)

The cast steel strip of claim 1, wherein the cooling rate is in the range of 100° C./sec to 300° C./sec.

### Claim 11 (depends on 1)

The cast steel strip of claim 1, wherein the finished cast steel strip has a yield strength of greater than 450 MPa.

### Claim 12 (depends on 2)

The cast steel strip of claim 2, wherein the final cast steel strip has a yield strength in the range of 450 MPa to 700 MPa.

### Claim 13 (depends on 12)

The cast steel strip of claim 12, wherein the cast steel has the following composition by weight:
7 Carbon 0.02-0.08% Manganese 0.30-0.80% Silicon 0.10-0.40% Sulfur 0.002-0.05% Aluminum less than 0.01%

### Claim 14

A cast steel strip prepared by a process comprising the steps of:
supporting a casting pool of molten low carbon steel on a pair of chilled casting rolls forming a nip between them and continuously casting solidified strip of no more than 5 mm in thickness and including austenite grains by rotating the rolls in mutually opposite directions such that the solidified strip moves downwardly from the nip;
passing the strip through a rolling mill in which the strip is hot rolled to produce a reduction in the strip thickness of at least 15%; and
continuously cooling the strip to transform the austenite to ferrite within a temperature range between 400° C. and 850° C. at a cooling rate of not less than 90° C./sec without inhibiting the cooling rate.

### Claim 15 (depends on 14)

The cast steel strip of claim 14, wherein said cooling rate is in the range 100° C./sec to 300° C./sec.

### Claim 16 (depends on 14)

The cast steel strip of claim 14, wherein the low carbon steel is a silicon/manganese killed steel having the following composition by weight:
8 Carbon 0.02-0.08% Manganese 0.30-0.80% Silicon 0.10-0.40% Sulfur 0.002-0.05% Aluminum less than 0.01%

### Claim 17 (depends on 14)

The cast steel strip of claim 14, wherein the low carbon steel is aluminum killed steel.

### Claim 18 (depends on 17)

The cast steel strip of claim 17, wherein the aluminum killed steel has the following composition by weight:
9 Carbon 0.02-0.08% Manganese 0.40% max Silicon 0.05% max Sulfur 0.002-0.05% Aluminum 0.05% max

### Claim 19 (depends on 14)

The cast steel strip of claim 14, wherein the finished strip has a yield strength of greater than 450 MPa.

### Claim 20 (depends on 14)

The cast steel strip of claim 14, wherein said cooling rate is in the range 100° C./sec to 300° C./sec and the strip has a yield strength of at least 450 MPa.

### Claim 21 (depends on 20)

The cast steel strip of claim 20, wherein the strip has a yield strength in the range of 450 MPa to 700 MPa.

### Claim 22 (depends on 14)

The cast steel strip of claim 14, wherein the low carbon steel is a silicon/manganese killed steel, and the strip is cooled at a cooling rate in the range of 100° C./sec to 300° C./sec to produce a strip having a yield strength of at least 450 MPa.

### Claim 23 (depends on 22)

The cast steel strip of claim 22, wherein the final strip has a yield strength in the range of 450 MPa to 700 MPa.

### Claim 24 (depends on 14)

The cast steel strip of claim 14, wherein the low carbon steel is a silicon/manganese killed steel, and the strip is hot rolled in the temperature range of 900° C. to 1100° C. and then is cooled at a cooling rate in the range of 100° C./sec to 300° C./sec to produce a final strip having a yield strength of at least 450 MPa.

### Claim 25 (depends on 24)

The cast steel strip of claim 24, wherein the final strip has a yield strength in the range of 450 MPa to 700 MPa.

### Claim 26 (depends on 24)

The cast steel strip of claim 24, wherein the steel has the following composition by weight:
10 Carbon 0.02-0.08% Manganese 0.30-0.80% Silicon 0.10-0.40% Sulfur 0.002-0.05% Aluminum less than 0.01%.