# US 2004/0079456 A1 · Copper alloy containing cobalt, nickel and silicon

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2004/0079456 A1
- Document ID: US20040079456A1
- Status: Published application
- Kind: A1
- Application number: 10/610,433
- Filed: 2003-06-30
- Published: 2004-04-29
- Earliest claimed: 2002-07-02
- Assignees: Onlin Corporation; Wieland-Werke AG
- Inventors: Frank N. Mandigo; Peter W. Robinson; Derek E. Tyler; Andreas Boegel; Hans-Achim Kuhn; Frank M. Keppeler; Joerg Seeger
- Web page: https://patentgrep.com/patent/US20040079456A1

## CPC

- C22F 1/08: of copper or alloys based thereon
- C22C 9/06: with nickel or cobalt as the next major constituent
- H01R 13/03: characterised by the material, e.g. plating, or coating materials
- H10W 70/456: {Materials}
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- H01R: ELECTRICALLY-CONDUCTIVE CONNECTIONS; STRUCTURAL ASSOCIATIONS OF A PLURALITY OF MUTUALLY-INSULATED ELECTRICAL CONNECTING ELEMENTS; COUPLING DEVICES; CURRENT COLLECTORS
- H10W: GENERIC PACKAGES, INTERCONNECTIONS, CONNECTORS OR OTHER CONSTRUCTIONAL DETAILS OF DEVICES COVERED BY CLASS H10

## Abstract

A copper alloy having an improved combination of yield strength and electrical conductivity consists essentially of, by weight, from 1% to 2.5% of nickel, from 0.5% to 2.0% of cobalt, with a total nickel plus cobalt content of from 1.7% to 4.3%, from 0.5% to 1.5% of silicon with a ratio of (Ni+Co)/Si of between 3.5 and 6, and the balance copper and inevitable impurities wherein the wrought copper alloy has an electrical conductivity in excess of 40% IACS. A further increase in the combination of yield strength and electrical conductivity as well as enhanced resistance to stress relaxation is obtained by a further inclusion of up 1% of silver. A process to manufacture the alloys of the invention as well as other copper-nickel-silicon alloys includes the sequential steps of (a). casting the copper alloy; (b). hot working the cast copper-base alloy to effect a first reduction in cross-sectional area; (c). solutionizing the cast copper-base alloy at a temperature and for a time effective to substantially form a single phase alloy; (d). first age annealing the alloy at a temperature and for a time effective to precipitate an amount of a second phase effective to form a multi-phase alloy having silicides; (e). cold working the multi-phase alloy to effect a second reduction in cross-sectional area; and (f). second age annealing the multiphase alloy at a temperature and for a time effective to precipitate additional silicides thereby raising conductivity, wherein the second age annealing temperature is less than the first age annealing temperature.

## Claims

### Claim 1

A wrought copper alloy consisting essentially, by weight, of:
from 1% to 2.5% of nickel;
from 0.5% to 2.0% of cobalt, with a total nickel plus cobalt content of from 1.7% to 4.3%;
from 0.5% to 1.5% of silicon with a ratio of (Ni+Co)/Si being between 2:1 and 7:1; and
the balance copper and inevitable impurities wherein said wrought copper alloy has an electrical conductivity in excess of 40% IACS.

### Claim 2 (depends on 1)

The wrought copper alloy of claim 1 wherein a maximum content of zinc is 0.25% and a maximum content of chromium is 0.08%.

### Claim 3 (depends on 2)

The wrought copper alloy of claim 2 wherein said nickel content is from 1.3% to 1.9%, said cobalt content is from 0.5% to 1.5% and said silicon content is from 0.5% to 0.8%.

### Claim 4 (depends on 3)

The wrought copper alloy of claim 3 wherein a weight percent ratio of nickel to cobalt is from 1.01:1 to 2.6:1.

### Claim 5 (depends on 4)

The wrought copper alloy of claim 4 wherein said wrought copper alloy has a yield strength of 100 ksi or greater.

### Claim 6 (depends on 1)

The copper alloy of claim 1 wherein an average grain size of said wrought copper alloy following solutionizing is 20 microns or less.

### Claim 7 (depends on 6)

The wrought copper alloy of claim 6 wherein a maximum content of zinc is 0.25% and a maximum content of chromium is 0.08%.

### Claim 8 (depends on 7)

The wrought copper alloy of claim 7 wherein said nickel content is from 1.3% to 1.9%, said cobalt content is from 0.5% to 1.5% and said silicon content is from 0.5% to 0.8%.

### Claim 9 (depends on 1)

The wrought copper alloy of claim 1 wherein said nickel content is from 1.3% to 1.9%, said cobalt content is from 0.5% to 1.5% and said silicon content is from 0.5% to 0.8%.

### Claim 10 (depends on 9)

The wrought copper alloy of claim 9 wherein a weight percent ratio of nickel to cobalt is from 1.01:1 to 2.6:1.

### Claim 11 (depends on 10)

The wrought copper alloy of claim 10 wherein a maximum content of zinc is 0.25% and a maximum content of chromium is 0.08%.

### Claim 12

A wrought copper alloy consisting essentially, by weight, of:
from 1% to 2.5% of nickel;
from 0.5% to 2.0% of cobalt, with a total nickel plus cobalt content of from 1.7% to 4.3%;
from 0.5% to 1.5% of silicon with a ratio of (Ni+Co)/Si being between 2:1 and 7:1;
from an amount effective to improve a combination of yield strength and electrical conductivity up to 1.0% of silver, titanium, zirconium and combinations thereof;
up to 0.15% of magnesium; and
the balance copper and inevitable impurities wherein said wrought copper alloy has an electrical conductivity in excess of 40% IACS.

### Claim 13 (depends on 12)

The wrought copper alloy of claim 12 wherein said silver content is from 0.2% to 0.7%.

### Claim 14 (depends on 13)

The wrought copper alloy of claim 13 wherein the magnesium content is between 0.005% and 0.04%, the maximum content of zinc is 0.25%, the maximum content of chromium is 0.08% and the maximum contents of each of tin and phosphorous is 0.04%.

### Claim 15 (depends on 14)

The wrought copper alloy of claim 14 wherein said nickel content is from 1.3% to 1.9%, said cobalt content is from 0.5% to 1.5% and said silicon content is from 0.5% to 0.8%.

### Claim 16 (depends on 15)

The wrought copper alloy of claim 15 wherein a weight percent ratio of nickel to cobalt is from 1.01:1 to 2.6:1.

### Claim 17 (depends on 16)

The wrought copper alloy of claim 16 wherein said wrought copper alloy has a yield strength of 100 ksi or greater.

### Claim 18 (depends on 13)

The copper alloy of claim 13 wherein an average grain size of said wrought copper alloy following solutionizing is 20 microns or less.

### Claim 19 (depends on 18)

The wrought copper alloy of claim 18 wherein the magnesium content is between 0.005% and 0.04%, the maximum content of zinc is 0.25%, the maximum content of chromium is 0.08% and the maximum contents of each of tin and phosphorous is 0.04%.

### Claim 20 (depends on 19)

The wrought copper alloy of claim 19 wherein said nickel content is from 1.3% to 1.9%, said cobalt content is from 0.5% to 1.5% and said silicon content is from 0.5% to 0.8%.

### Claim 21 (depends on 13)

The wrought copper alloy of claim 13 wherein said nickel content is from 1.3% to 1.9%, said cobalt content is from 0.5% to 1.5% and said silicon content is from 0.5% to 0.8%.

### Claim 22 (depends on 21)

The wrought copper alloy of claim 21 wherein a weight percent ratio of nickel to cobalt is from 1.01:1 to 2.6:1.

### Claim 23 (depends on 22)

The wrought copper alloy of claim 22 wherein the magnesium content is between 0.005% and 0.04%, the maximum content of zinc is 0.25%, the maximum content of chromium is 0.08% and the maximum contents of each of tin and phosphorous is 0.04%.

### Claim 24

A process for the manufacture of a copper-base alloy, comprising the sequential steps of:
a). casting said copper-base alloy containing, by weight, from 0.5% to 5.0% nickel and 0.1% to 1.5% silicon;
b). hot working said cast copper-base alloy to effect a first reduction in cross-sectional area;
c). solutionizing said cast copper-base alloy at a solutionizing temperature and for a first time effective to substantially form a single phase alloy;
d). without any intervening cold work following said solutionizing, first age annealing said substantially single phase alloy at a first age anneal temperature and for a second time effective to precipitate a second phase;
e). cold working said multi-phase alloy to effect a second reduction in cross-sectional area; and
f). second age annealing said multiphase alloy at a second age anneal temperature and for a third time effective to precipitate an additional amount of said second phase, wherein said second age anneal temperature is less than said first age anneal temperature.

### Claim 25 (depends on 24)

The process of claim 24 wherein following said solutionizing step, an average grain size of said wrought copper alloy is 20 microns or less.

### Claim 26 (depends on 24)

The process of claim 24 including a step of cold working said wrought copper alloy between said hot working step (b) and said solutionizing step (c).

### Claim 27 (depends on 26)

The process of claim 26 wherein both said hot working step and said cold working steps constitute rolling and said wrought copper alloy is formed into a strip.

### Claim 28

A process for the manufacture of a copper-base alloy, comprising the sequential steps of:
a). casting said copper-base alloy containing, by weight, from 0.5% to 5.0% nickel and 0.1% to 1.5% silicon;
b). hot working said cast copper-base alloy in one or more passes to form a hot worked product;
c). solutionizing said hot worked product at a temperature in excess of from 800° C. to a solidus temperature of said copper-base alloy;
d). without any intervening cold work following said solutionizing, first age annealing said hot worked plate at a temperature of from 350° C. to 600° C. for from 30 minutes to 30 hours;
e). cold working said hot worked plate to a reduction in cross-sectional area of from 10% to 50% to form a product; and
f). second age annealing said product at a temperature less than said first precipitation annealing temperature.

### Claim 29 (depends on 28)

The process of claim 28 wherein said hot working is at a temperature of between 850° C. and 1000° C. and said solutionizing temperature of between 800° C. and 1000° C.

### Claim 30 (depends on 29)

The process of claim 29 further including a step of quenching said copper base alloy following said hot working step (b).

### Claim 31 (depends on 30)

The process of claim 30 wherein said first age anneal is at a temperature of between 475° C. and 550° C. and said second age anneal temperature is between 350° C. and 500° C.

### Claim 32 (depends on 31)

The process of claim 31 further including a step of cold working said copper alloy to a gauge effective for solutionizing between said quench and said solutionizing step (c).

### Claim 33 (depends on 32)

The process of claim 32 wherein said hot working step and said cold working steps both constitute rolling thereby forming said copper alloy into a strip.

### Claim 34 (depends on 32)

The process of claim 32 wherein said copper alloy is selected to have a composition of from 1% to 2.5% of nickel, from 0.5% to 2.0% of cobalt, with a total nickel plus cobalt content of from 1.7% to 4.3%, from 0.5% to 1.5% of silicon with a ratio of (Ni+Co)/Si being between 2:1 and 7:1 and the balance copper and inevitable impurities.

### Claim 35 (depends on 32)

The process of claim 32 wherein said copper alloy is selected to have a composition of from 1% to 2.5% of nickel, from 0.5% to 2.0% of cobalt, with a total nickel plus cobalt content of from 1.7% to 4.3%, from 0.5% to 1.5% of silicon with a ratio of (Ni+Co)/Si being between 2:1 and 7:1, from an amount effective to improve a combination of yield strength and electrical conductivity up to 1.0% of silver, titanium, zirconium and combinations thereof, up to 0.15% of magnesium and the balance copper and inevitable impurities

### Claim 36 (depends on 32)

The process of claim 32 wherein said copper alloy is selected to have a composition of 2.2%-4.2% nickel, 0.25%-1.2% silicon, 0.05%-0.30% magnesium and the balance copper.

### Claim 37

A process for the manufacture of a copper-base alloy, comprising the sequential steps of:
a). casting said copper-base alloy containing, by weight, from 0.5% to 5.0% nickel and 0.1% to 1.5% silicon;
b). hot working said cast copper-base alloy in one or more passes to form a hot worked product;
c). first age annealing said hot worked product at a temperature of from 350° C. to 600° C. for from 30 minutes to 30 hours;
d). cold working said hot worked product to a reduction in cross-sectional area of from 10% to 50% to form a product; and
e). second age annealing said product at a temperature less than said first precipitation annealing temperature.

### Claim 38 (depends on 37)

The process of claim 37 wherein said hot working is at a temperature of between 850° C. and 1000° C.

### Claim 39 (depends on 38)

The process of claim 38 further including a step of quenching said copper base alloy following said hot working step (b).

### Claim 40 (depends on 39)

The process of claim 39 wherein said first age anneal is at a temperature of between 475° C. and 550° C. and said second age anneal temperature is between 350° C. and 500° C.

### Claim 41 (depends on 40)

The process of claim 40 wherein said copper alloy is selected to have a composition of from 1% to 2.5% of nickel, from 0.5% to 2.0% of cobalt, with a total nickel plus cobalt content of from 1.7% to 4.3%, from 0.5% to 1% of silicon with a ratio of (Ni+Co)/Si being between 3.5 and 5.5 and the balance copper and inevitable impurities.

### Claim 42 (depends on 40)

The process of claim 40 wherein said copper alloy is selected to have a composition of from 1% to 2.5% of nickel, from 0.5% to 2.0% of cobalt, with a total nickel plus cobalt content of from 1.7% to 4.3%, from 0.5% to 1.5% of silicon with a ratio of (Ni+Co)/Si being between 2:1 and 7: 1, from an amount effective to improve a combination of yield strength and electrical conductivity up to 1.0% of silver, titanium, zirconium and combinations thereof, up to 0.15% of magnesium and the balance copper and inevitable impurities

### Claim 43 (depends on 37)

The process of claim 37 further including a step of cold working between said hot working step (b) and said first age annealing step (c).

### Claim 44 (depends on 37)

The process of claim 37 wherein there is no intervening cold working between said hot working step (b and said first age annealing step (c).

### Claim 45

A processes for the manufacture of a copper-base alloy, comprising the sequential steps of:
a). casting said copper-base alloy containing, by weight, from 0.5% to 5.0% nickel and 0.1% to 1.5% silicon;
b). hot working said cast copper-base alloy in one or more passes to form a hot worked product;
c). solutionizing said hot worked product at a temperature in excess of from 800° C. to a solidus temperature of said copper-base alloy;
d). cold working said copper base alloy for a reduction in cross-sectional area;
e). first age annealing said hot worked plate at a temperature of from 350° C. to 600° C. for from 30 minutes to 30 hours;
f). cold working said hot worked plate to a reduction in cross-sectional area of from 10% to 50% to form a product; and
g). second age annealing said product at a temperature less than said first precipitation annealing temperature.

### Claim 46 (depends on 45)

The process of claim 45 wherein said hot working is at a temperature of between 850° C. and 1000° C. and said solutionizing temperature if between 800° C. and 1000° C.

### Claim 47 (depends on 46)

The process of claim 46 further including a step of quenching said copper base alloy following said hot working step (b).

### Claim 48 (depends on 47)

The process of claim 47 wherein said first age anneal is at a temperature of between 475° C. and 550° C. and said second age anneal temperature is between 350° C. and 500° C.

### Claim 49 (depends on 48)

The process of claim 48 further including a step of cold working said copper alloy to a gauge effective for solutionizing between said quench and said solutionizing step (c).

### Claim 50 (depends on 49)

The process of claim 49 wherein said hot working step and said cold working steps both constitute rolling thereby forming said copper alloy into a strip.

### Claim 51 (depends on 49)

The process of claim 49 wherein said copper alloy is selected to have a composition of from 1% to 2.5% of nickel, from 0.5% to 2.0% of cobalt, with a total nickel plus cobalt content of from 1.7% to 4.3%, from 0.5% to 1.5% of silicon with a ratio of (Ni+Co)/Si being between 2:1 and 7:1 and the balance copper and inevitable impurities.

### Claim 52 (depends on 49)

The process of claim 49 wherein said copper alloy is selected to have a composition of from 1% to 2.5% of nickel, from 0.5% to 2.0% of cobalt, with a total nickel plus cobalt content of from 1.7% to 4.3%, from 0.5% to 1.5% of silicon with a ratio of (Ni+Co)/Si being between 2:1 and 7:1, from an amount effective to improve a combination of yield strength and electrical conductivity up to 1.0% of silver, titanium, zirconium and combinations thereof, up to 0.15% of magnesium and the balance copper and inevitable impurities

### Claim 53 (depends on 49)

The process of claim 49 wherein said copper alloy is selected to have a composition of 2.2%-4.2% nickel, 0.25%-1.2% silicon, 0.05%-0.30% magnesium and the balance copper.

### Claim 54

A processes for the manufacture of a copper-base alloy, comprising the sequential steps of:
a). casting said copper-base alloy containing from 0.35% to 5% of titanium and 0.001% to 5% X, where X is selected from Ni, Fe, Sn, P, Al, Zn, Si, Pb, Be, Mn, Mg, Bi, S, Te, Se, Ag, As, Sb, Zr, B, Cr and Co and combinations thereof;
b). hot working said cast copper-base alloy in one or more passes to form a hot worked product;
c). solutionizing said hot worked product at a temperature in excess of from 800° C. to a solidus temperature of said copper-base alloy;
d). cold working said copper base alloy for a reduction in cross-sectional area;
e). first age annealing said hot worked plate at a temperature of from 350° C. to 600° C. for from 30 minutes to 30 hours;
f). cold working said hot worked plate to a reduction in cross-sectional area of from 10% to 50% to form a product; and
g). second age annealing said product at a temperature less than said first precipitation annealing temperature.

### Claim 55 (depends on 54)

The process of claim 54 wherein said hot working is at a temperature of between 850° C. and 1000° C. and said solutionizing temperature if between 800° C. and 1000° C.

### Claim 56 (depends on 55)

The process of claim 55 further including a step of quenching said copper base alloy following said hot working step (b).

### Claim 57 (depends on 56)

The process of claim 56 wherein said first age anneal is at a temperature of between 475° C. and 550° C. and said second age anneal temperature is between 350° C. and 500° C.

### Claim 58 (depends on 57)

The process of claim 57 further including a step of cold working said copper alloy to a gauge effective for solutionizing between said quench and said solutionizing step (c).

### Claim 59 (depends on 58)

The process of claim 58 wherein said hot working step and said cold working steps both constitute rolling thereby forming said copper alloy into a strip.