# US 2004/0079455 A1 · AlCuMg alloys with high damage tolerance suitable for use as structural members in aircrafts

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2004/0079455 A1
- Document ID: US20040079455A1
- Status: Published application
- Kind: A1
- Application number: 10/614,888
- Filed: 2003-07-09
- Published: 2004-04-29
- Earliest claimed: 2002-07-09
- Assignees: Pechiney Rhenalu
- Inventors: Ronan Dif; Timothy Warner; Bernard Bes
- Web page: https://patentgrep.com/patent/US20040079455A1

## CPC

- C22F 1/053: of alloys with zinc as the next major constituent
- C22C 21/16: with magnesium
- C22F 1/057: of alloys with copper as the next major constituent
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

New alloys for potential use in applications such as in lower wing skins and fuselage skins are disclosed. Specifically, Mn-free 2×24 alloys potentially suitable for thick plate and thin plate and sheet applications are believed to be novel and to provide unexpectedly superior properties.

## Claims

### Claim 1

A substantially manganese-free aluminum alloy rolled product consisting essentially of (in percent by weight): Cu 3.6-4.5%, Mg 1.0-1.6%, Zr 0.08-0.20%, Sc up to 0.06%, Fe up to 0.08%, Si up to 0.09%, Mn less than 0.05%,remainder aluminum and incident impurities.

### Claim 2 (depends on 1)

An aluminum alloy rolled product according to claim 1, wherein Sc is present in an amount from 0.02-0.05%.

### Claim 3 (depends on 1)

An aluminum alloy rolled product according to claim 1, wherein Zr is present in an amount from 0.08-0.14%.

### Claim 4 (depends on 1)

An aluminum alloy rolled product according to claim 1, wherein Cu is present in an amount from 0.10-0.14%.

### Claim 5 (depends on 1)

An aluminum alloy rolled product according to claim 1, having a recrystallized volume fraction of 5% maximum.

### Claim 6 (depends on 1)

An aluminum alloy rolled product according to claim 1, wherein Mn is present in an amount of <0.01%.

### Claim 7 (depends on 1)

An aluminum alloy rolled product according to claim 1, having one or more of the following combinations of properties:
a. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 400 MPa, and an apparent fracture toughness Kapp(T-L) of more than 110 MPa{square root}m, measured according to ASTM E 561 in the T-L orientation on a specimen with a width of W=127 mm;
b. an ultimate tensile strength in the longitudinal direction (UTS(L)) of more than 450 MPa, and an elongation at fracture in the longitudinal direction of more than 24%;
c. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 400 MPa, and a Kahn stress Re of at least 180 MPa.

### Claim 8 (depends on 1)

An aluminum alloy rolled product according to claim 1 comprising a sheet having on or more of the following combinations of properties :
a. a UTS(L) of more than 500 MPa, preferably more than 520 Mpa, and even more preferably more than 530 Mpa, and a Kapp(T-L) of more than 75 Mpa{square root}m, measured according to ASTM E 647 on a 6.35 mm thick C(T) specimen with a width of W=40 mm;
b. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 450 Mpa, and preferably more than 460 Mpa, and a Kapp(L-T) of more than 77 Mpa{square root}m, measured according to ASTM E 561 on a 6.35 mm thick C(T) specimen with a width of W=40 mm;
c. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 350 MPa, preferably more than 400 MPa and even more preferably more than 450 MPa, and a Kahn stress Re of at least 190 MPa.

### Claim 9 (depends on 1)

An aluminum alloy rolled product according to claim 1, comprising a sheet or thin plate with a thickness below about 12 mm in T351 temper, having a da/dn in T-L direction which fulfils at least one of the following conditions:
da/dn less than 1.3 10−4 mm/cycles at ΔK=10 MPa{square root}m,
da/dn less than 4.0 10−4 mm/cycles at ΔK=15 MPa{square root}m,
da/dn less than 8.0 10−4 mm/cycles at ΔK=20 MPa{square root}m,
da/dn less than 16 10−4 mm/cycles at ΔK=25 MPa{square root}m,
da/dn less than 25 10−4 mm/cycles at ΔK=30 MPa{square root}m.

### Claim 10 (depends on 1)

An aluminum alloy rolled product according to claim 1 comprising a plate in T351 temper having a da/dn in T-L direction which fulfils at least one of the following conditions:
da/dn less than 3.0 10−5 mm/cycles at ΔK=10 MPa{square root}m,
da/dn less than 1.0 10−4 mm/cycles at ΔK=15 MPa{square root}m,
da/dn less than 1.0 10−3 mm/cycles at ΔK=25 MPa{square root}m,
da/dn less than 3 10−3 mm/cycles at ΔK=30 MPa{square root}m.

### Claim 11 (depends on 1)

An aluminum alloy rolled product according to claim 1, exhibiting in a corrosion test according to ASTM G 110, a maximum intergranular attack of less than 80 μm in T39 temper, and/or less than 200 μm in T851 temper, and/or less than 250 μm in T89 temper, and/or less than 300 μm in T351 temper.

### Claim 12 (depends on 1)

An aluminum alloy rolled product according to claim 1, exhibiting in a corrosion test according to ASTM G 110 a maximum intergranular attack of less than 70 μm in T39 temper, and/or less than 180 μm in T851 temper, and/or less than 220 μm in T89 temper, and/or less than 270 μm in T351 temper.

### Claim 13 (depends on 1)

A lower wing skin structural member made in an aluminum alloy rolled plate product according to claim 1.

### Claim 14 (depends on 1)

A fuselage skin member made in an aluminum alloy rolled plate or sheet product according to claim 1.

### Claim 15 (depends on 1)

A method for obtaining an aluminum alloy rolled product according to claim 1, wherein said rolled product comprises a plate, said method comprising:
(a) Casting a rolling ingot, followed by optional stress relieving ,and scalping,
(b) Homogenizing at a temperature between 450 and 510° C.,
(c) Hot-rolling on a reversing mill, preferably with an exit temperature between 350 and 390° C.,
(d) Optionally, for plate with a thickness of less than about 30 mm, conducting at least one intermediate reheating to about 480° C., followed by one or more hot-rolling passes, the final exit temperature optionally being between 350 and 370° C.,
(e) Solution heat treating at a temperature between 490 and 510° C., followed by water quenching and natural aging,
(f) Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 16 (depends on 1)

A method for obtaining a rolled product according to claim 1 comprising a sheet product, said method comprising:
(a) Casting a rolling ingot, followed by optional stress relieving, and scalping,
(b) Homogenizing at a temperature between 470 and 530° C.,
(c) Hot-rolling down to a thickness of less than 12 mm, and not more than 200% of final thickness, with a final exit temperature between 230 and 350° C.,
(d) Optionally cold rolling,
(e) Solution heat treating at a temperature between 490 and 510° C., followed by water quenching,
(f) Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 17

An alloy comprising a composition selected from the group consisting of: (in weight %)
18 Si Fe Cu Mn Mg Ti Zr Sc <0.06 0.06 4.12 0.40 1.37 0.022 <0.06 0.06 3.81 0.008 1.41 0.022 0.109 <0.06 0.07 3.81 0.008 1.36 0.024 0.107 0.028 <0.06 0.05 4.20 0.24 1.23 0.016 0.11 0.032 <0.06 0.06 4.14 0.51 1.24 0.019 0.11 0.032

### Claim 18

A substantially manganese-free aluminum alloy rolled product comprising (in percent by weight): Cu 3.6-4.5%, Mg 1.0-1.6%, Zr 0.08-0.20%, Sc up to 0.06%, Fe up to 0.08%, Si up to 0.09%, Mn less than 0.05%,remainder aluminum and incident impurities.

### Claim 19 (depends on 2)

An aluminum alloy rolled product according to claim 2, wherein Zr is present in an amount from 0.08-0.14%.

### Claim 20 (depends on 2)

An aluminum alloy rolled product according to claim 2, wherein Cu is present in an amount from 0.10-0.14%.

### Claim 21 (depends on 3)

An aluminum alloy rolled product according to claim 3, wherein Cu is present in an amount from 0.10-0.14%.

### Claim 22 (depends on 2)

An aluminum alloy rolled product according to claim 2, having a recrystallized volume fraction of 5% maximum.

### Claim 23 (depends on 3)

An aluminum alloy rolled product according to claim 3 having a recrystallized volume fraction of 5% maximum.

### Claim 24 (depends on 4)

An aluminum alloy rolled product according to claim 4 having a recrystallized volume fraction of 5% maximum.

### Claim 25 (depends on 2)

An aluminum alloy rolled product according to claim 2, wherein Mn is present in an amount of <0.01%.

### Claim 26 (depends on 3)

An aluminum alloy rolled product according to claim 3, wherein Mn is present in an amount of <0.01%.

### Claim 27 (depends on 4)

An aluminum alloy rolled product according to claim 4, wherein Mn is present in an amount of<0.01%.

### Claim 28 (depends on 5)

An aluminum alloy rolled product according to claim 5, wherein Mn is present in an amount of <0.01%.

### Claim 29 (depends on 2)

An aluminum alloy rolled product according to claim 2, having one or more of the following combinations of properties:
a. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 400 MPa, and an apparent fracture toughness Kapp(T-L) of more than 110 MPa{square root}m, measured according to ASTM E 561 in the T-L orientation on a specimen with a width of W=127 mm;
b. an ultimate tensile strength in the longitudinal direction (UTS(L)) of more than 450 MPa, and an elongation at fracture in the longitudinal direction of more than 24%;
c. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 400 MPa, and a Kahn stress Re of at least 180 MPa, and preferably at least 190 MPa.

### Claim 30 (depends on 3)

An aluminum alloy rolled product according to claim 3, having one or more of the following combinations of properties:
a. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 400 MPa, and an apparent fracture toughness Kapp(T-L) of more than 110 MPa{square root}m, measured according to ASTM E 561 in the T-L orientation on a specimen with a width of W=127 mm;
b. an ultimate tensile strength in the longitudinal direction (UTS(L)) of more than 450 MPa, and an elongation at fracture in the longitudinal direction of more than 24%;
c. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 400 MPa, and a Kahn stress Re of at least 180 MPa.

### Claim 31 (depends on 3)

An aluminum alloy rolled product according to claim 3, having one or more of the following combinations of properties:
a. tensile yield strength in the longitudinal direction (TYS(L)) of more than 400 MPa, and an apparent fracture toughness Kapp(TL) of more than 110 MPa{square root}m, measured according to ASTM E 561 in the T-L orientation on a specimen with a width of W=127 mm;
b. an ultimate tensile strength in the longitudinal direction (UTS(L)) of more than 450 MPa, and an elongation at fracture in the longitudinal direction of more than 24%;
c. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 400 MPa, and a Kahn stress Re of at least 180 MPa..

### Claim 32 (depends on 2)

An aluminum alloy rolled product according to claim 2 comprising a plate having on or more of the following combinations of properties:
a. a UTS(L) of more than 500 MPa, and a Kapp(T-L) of more than 75 MPa{square root}m, measured according to ASTM E 647 on a 6.35 mm thick C(T) specimen with a width of W=40 mm;
b. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 450 MPa, and a Kapp(L-T) of more than 77 MPa{square root}m, measured according to ASTM E 561 on a 6.35 mm thick C(T) specimen with a width of W=40 mm;
c. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 350 MPa, and a Kahn stress Re of at least 190 MPa.

### Claim 33 (depends on 3)

An aluminum alloy rolled product according to claim 3 comprising a plate having on or more of the following combinations of properties:
a. a UTS(L) of more than 500 MPa, and a Kapp(T-L) of more than 75 MPa{square root}m, measured according to ASTM E 647 on a 6.35 mm thick C(T) specimen with a width of W=40 mm;
b. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 450 MPa, and a Kapp(L-T) of more than 77 MPa{square root}m, measured according to ASTM E 561 on a 6.35 mm thick C(T) specimen with a width of W=40 mm;
c. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 350 MPa, and a Kahn stress Re of at least 190 MPa.

### Claim 34 (depends on 4)

An aluminum alloy rolled product according to claim 4 comprising a plate having on or more of the following combinations of properties:
a. a UTS(L) of more than 500 MPa, and a Kapp(T-L) of more than 75 MPa{square root}m, measured according to ASTM E 647 on a 6.35 mm thick C(T) specimen with a width of W=40 mm;
b. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 450 MPa, and a Kapp(L-T) of more than 77 MPa{square root}m, measured according to ASTM E 561 on a 6.35 mm thick C(T) specimen with a width of W=40 mm;
c. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 350 MPa, and a Kahn stress Re of at least 190 MPa.

### Claim 35 (depends on 5)

An aluminum alloy rolled product according to claim 5 comprising a plate having on or more of the following combinations of properties:
a. a UTS(L) of more than 500 MPa, and a Kapp(T-L) of more than 75 MPa{square root}m, measured according to ASTM E 647 on a 6.35 mm thick C(T) specimen with a width of W=40 mm;
b. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 450 MPa, and a Kapp(L-T) of more than 77 MPa{square root}m, measured according to ASTM E 561 on a 6.35 mm thick C(T) specimen with a width of W=40 mm;
c. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 350 MPa, and a Kahn stress Re of at least 190 MPa.

### Claim 36 (depends on 6)

An aluminum alloy rolled product according to claim 6 comprising a plate having on or more of the following combinations of properties:
a. a UTS(L) of more than 500 MPa, and a Kapp(T-L) of more than 75 MPa{square root}m, measured according to ASTM E 647 on a 6.35 mm thick C(T) specimen with a width of W=40 mm;
b. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 450 MPa, and a Kapp(L-T) of more than 77 MPa{square root}m, measured according to ASTM E 561 on a 6.35 mm thick C(T) specimen with a width of W=40 mm;
c. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 350 MPa, and a Kahn stress Re of at least 190 MPa.

### Claim 37 (depends on 7)

An aluminum alloy rolled product according to claim 7 comprising a plate having on or more of the following combinations of properties:
a. a UTS(L) of more than 500 MPa, and a Kapp(T-L) of more than 75 MPa{square root}m, measured according to ASTM E 647 on a 6.35 mm thick C(T) specimen with a width of W=40 mm;
b. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 450 MPa, and a Kapp(L-T) of more than 77 MPa{square root}m, measured according to ASTM E 561 on a 6.35 mm thick C(T) specimen with a width of W=40 mm;
c. a tensile yield strength in the longitudinal direction (TYS(L)) of more than 350 MPa, and a Kahn stress Re of at least 190 MPa.

### Claim 38 (depends on 2)

An aluminum alloy rolled product according to claim 2 comprising a sheet or thin plate with a thickness below about 12 mm in T351 temper having a da/dn in T-L direction which fulfils at least one of the following conditions:
da/dn less than 1.3 10−4 mm/cycles at ΔK=10 MPa{square root}m,
da/dn less than 4.0 10−4 mm/cycles at ΔK=15 MPa{square root}m,
da/dn less than 8.0 10−4 mm/cycles at ΔK=20 MPa{square root}m,
da/dn less than 16 10−4 mm/cycles at ΔK=25 MPa{square root}m,
da/dn less than 25 10−4 mm/cycles at ΔK=30 MPa{square root}m.

### Claim 39 (depends on 3)

An aluminum alloy rolled product according to claim 3, comprising a sheet or thin plate with a thickness below about 12 mm in T351 temper having a da/dn in T-L direction which fulfils at least one of the following conditions:
da/dn less than 1.3 10−4 mm/cycles at ΔK=10 MPa{square root}m,
da/dn less than 4.0 10−4 mm/cycles at ΔK=15 MPa{square root}m,
da/dn less than 8.0 10−4 mm/cycles at ΔK=20 MPa{square root}m,
da/dn less than 16 10−4 mm/cycles at ΔK=25 MPa{square root}m,
da/dn less than 25 10−4 mm/cycles at ΔK=30 MPa{square root}m.

### Claim 40 (depends on 4)

An aluminum alloy rolled product according to claim 4 comprising a sheet or thin plate with a thickness below about 12 mm in T351 temper having a da/dn in T-L direction which fulfils at least one of the following conditions:
da/dn less than 1.3 10−4 mm/cycles at ΔK=10 MPa{square root}m,
da/dn less than 4.0 10−4 mm/cycles at ΔK=15 MPa{square root}m,
da/dn less than 8.0 10−4 mm/cycles at ΔK=20 MPa{square root}m,
da/dn less than 16 10−4 mm/cycles at ΔK=25 MPa{square root}m,
da/dn less than 25 10−4 mm/cycles at ΔK=30 MPa{square root}m.

### Claim 41 (depends on 5)

An aluminum alloy rolled product according to claim 5 comprising a sheet or thin plate with a thickness below about 12 mm in T351 temper having a da/dn in T-L direction which fulfils at least one of the following conditions:
da/dn less than 1.3 10−4 mm/cycles at ΔK=10 MPa{square root}m,
da/dn less than 4.0 10−4 mm/cycles at ΔK=15 MPa{square root}m,
da/dn less than 8.0 10−4 mm/cycles at ΔK=20 MPa{square root}m,
da/dn less than 16 10−4 mm/cycles at ΔK=25 MPa{square root}m,
da/dn less than 25 10−4 mm/cycles at ΔK=30 MPa{square root}m.

### Claim 42 (depends on 6)

An aluminum alloy rolled product according to claim 6 comprising a sheet or thin plate with a thickness below about 12 mm in T351 temper having a da/dn in T-L direction which fulfils at least one of the following conditions:
da/dn less than 1.3 10−4 mm/cycles at ΔK=10 MPa{square root}m,
da/dn less than 4.0 10−4 mm/cycles at ΔK=15 MPa{square root}m,
da/dn less than 8.0 10−4 mm/cycles at ΔK=20 MPa{square root}m,
da/dn less than 16 10−4 mm/cycles at ΔK=25 MPa{square root}m,
da/dn less than 25 10−4 mm/cycles at ΔK=30 MPa{square root}m.

### Claim 43 (depends on 7)

An aluminum alloy rolled product according to claim 7 comprising a sheet or thin plate with a thickness below about 12 mm in T351 temper having a da/dn in T-L direction which fulfils at least one of the following conditions:
da/dn less than 1.3 10−4 mm/cycles at ΔK=10 MPa{square root}m,
da/dn less than 4.0 10−4 mm/cycles at ΔK=15 MPa{square root}m,
da/dn less than 8.0 10−4 mm/cycles at ΔK=20 MPa{square root}m,
da/dn less than 16 10−4 mm/cycles at ΔK=25 MPa{square root}m,
da/dn less than 25 10−4 mm/cycles at ΔK=30 MPa{square root}m.

### Claim 44 (depends on 8)

An aluminum alloy rolled product according to claim 8 comprising a sheet or thin plate with a thickness below about 12 mm in T351 temper having a da/dn in T-L direction which fulfils at least one of the following conditions:
da/dn less than 1.3 10−4 mm/cycles at ΔK=10 MPa{square root}m,
da/dn less than 4.0 10−4 mm/cycles at ΔK=15 MPa{square root}m,
da/dn less than 8.0 10−4 mm/cycles at ΔK=20 MPa{square root}m,
da/dn less than 16 10−4 mm/cycles at ΔK=25 MPa{square root}m,
da/dn less than 25 10−4 mm/cycles at ΔK=30 MPa{square root}m.

### Claim 45 (depends on 2)

An aluminum alloy rolled product according to claim 2 comprising a plate in T351 temper having a da/dn in T-L direction which fulfils at least one of the following conditions:
da/dn less than 3.0 10−5 mm/cycles at ΔK=10 MPa{square root}m,
da/dn less than 1.0 10−4 mm/cycles at ΔK=15 MPa{square root}m,
da/dn less than 1.0 10−3 mm/cycles at ΔK=25 MPa{square root}m,
da/dn less than 3 10−3 mm/cycles at ΔK=30 MPa{square root}m.

### Claim 46 (depends on 3)

An aluminum alloy rolled product according to claim 3 comprising a plate in T351 temper having a da/dn in T-L direction which fulfils at least one of the following conditions:
da/dn less than 3.0 10−5 mm/cycles at ΔK=10 MPa{square root}m,
da/dn less than 1.0 10−4 mm/cycles at ΔK=15 MPa{square root}m,
da/dn less than 1.0 10−3 mm/cycles at ΔK=25 MPa{square root}m,
da/dn less than 3 10−3 mm/cycles at ΔK=30 MPa{square root}m.

### Claim 47 (depends on 4)

An aluminum alloy rolled product according to claim 4 comprising a plate in T351 temper having a da/dn in T-L direction which fulfils at least one of the following conditions:
da/dn less than 3.0 10−5 mm/cycles at ΔK=10 MPa{square root}m,
da/dn less than 1.0 10−4 mm/cycles at ΔK=15 MPa{square root}m,
da/dn less than 1.0 10−3 mm/cycles at ΔK=25 MPa{square root}m,
da/dn less than 3 10−3 mm/cycles at ΔK=30 MPa{square root}m.

### Claim 48 (depends on 5)

An aluminum alloy rolled product according to claim 5, comprising a plate in T351 temper having a da/dn in T-L direction which fulfils at least one of the following conditions:
da/dn less than 3.0 10−5 mm/cycles at ΔK=10 MPa{square root}m,
da/dn less than 1.0 10−4 mm/cycles at ΔK=15 MPa{square root}m,
da/dn less than 1.0 10−3 mm/cycles at ΔK=25 MPa{square root}m,
da/dn less than 3 10−3 mm/cycles at ΔK=30 MPa{square root}m.

### Claim 49 (depends on 6)

An aluminum alloy rolled product according to claim 6 comprising a plate in T351 temper having a da/dn in T-L direction which fulfils at least one of the following conditions:
da/dn less than 3.0 10−5 mm/cycles at ΔK=10 MPa{square root}m,
da/dn less than 1.0 10−4 mm/cycles at ΔK=15 MPa{square root}m,
da/dn less than 1.0 10−3 mm/cycles at ΔK=25 MPa{square root}m,
da/dn less than 3 10−3 mm/cycles at ΔK=30 MPa{square root}m.

### Claim 50 (depends on 7)

An aluminum alloy rolled product according to claim 7 comprising a plate in T351 temper, having a da/dn in T-L direction which fulfils at least one of the following conditions
da/dn less than 3.0 10−5 mm/cycles at ΔK=10 MPa{square root}m,
da/dn less than 1.0 10−4 mm/cycles at ΔK=15 MPa{square root}m,
da/dn less than 1.0 10−3 mm/cycles at ΔK=25 MPa{square root}m,
da/dn less than 3 10−3 mm/cycles at ΔK=30 MPa{square root}m.

### Claim 51 (depends on 8)

An aluminum alloy rolled product according to claim 8 comprising a plate in T351 temper having a da/dn in T-L direction which fulfils at least one of the following conditions
da/dn less than 3.0 10−5 mm/cycles at ΔK=10 MPa{square root}m,
da/dn less than 1.0 10−4 mm/cycles at ΔK=15 MPa{square root}m,
da/dn less than 1.0 10−3 mm/cycles at ΔK=25 MPa{square root}m,
da/dn less than 3 10−3 mm/cycles at ΔK=30 MPa{square root}m.

### Claim 52 (depends on 2)

An aluminum alloy rolled product according to claim 2, exhibiting in a corrosion test according to ASTM G 110, a maximum intergranular attack of less than 80 μm in T39 temper, and/or less than 200 μm in T851 temper, and/or less than 250 μm in T89 temper, and/or less than 300 μm in T351 temper.

### Claim 53 (depends on 3)

An aluminum alloy rolled product according to claim 3, exhibiting in a corrosion test according to ASTM G 110, a maximum intergranular attack of less than 80 μm in T39 temper, and/or less than 200 μm in T851 temper, and/or less than 250 μm in T89 temper, and/or less than 300 μm in T351 temper.

### Claim 54 (depends on 4)

An aluminum alloy rolled product according to claim 4, exhibiting in a corrosion test according to ASTM G 110, a maximum intergranular attack of less than 80 μm in T39 temper, and/or less than 200 μm in T851 temper, and/or less than 250 μm in T89 temper, and/or less than 300 μm in T351 temper.

### Claim 55 (depends on 5)

An aluminum alloy rolled product according to claim 5, exhibiting in a corrosion test according to ASTM G 110, a maximum intergranular attack of less than 80 μm in T39 temper, and/or less than 200 μm in T851 temper, and/or less than 250 μm in T89 temper, and/or less than 300 μm in T351 temper.

### Claim 56 (depends on 6)

An aluminum alloy rolled product according to claim 6, exhibiting in a corrosion test according to ASTM G 110, a maximum intergranular attack of less than 80 μm in T39 temper, and/or less than 200 μm in T851 temper, and/or less than 250 μm in T89 temper, and/or less than 300 μm in T351 temper.

### Claim 57 (depends on 7)

An aluminum alloy rolled product according to claim 7, exhibiting in a corrosion test according to ASTM G 110, a maximum intergranular attack of less than 80 μm in T39 temper, and/or less than 200 μm in T851 temper, and/or less than 250 μm in T89 temper, and/or less than 300 μm in T351 temper.

### Claim 58 (depends on 8)

An aluminum alloy rolled product according to claim 8, exhibiting in a corrosion test according to ASTM G 110, a maximum intergranular attack of less than 80 μm in T39 temper, and/or less than 200 μm in T851 temper, and/or less than 250 μm in T89 temper, and/or less than 300 μm in T351 temper.

### Claim 59 (depends on 9)

An aluminum alloy rolled product according to claim 9, exhibiting in a corrosion test according to ASTM G 110, a maximum intergranular attack of less than 80 μm in T39 temper, and/or less than 200 μm in T851 temper, and/or less than 250 μm in T89 temper, and/or less than 300 μm in T351 temper.

### Claim 60 (depends on 10)

An aluminum alloy rolled product according to claim 10, exhibiting in a corrosion test according to ASTM G 110, a maximum intergranular attack of less than 80 μm in T39 temper, and/or less than 200 μm in T851 temper, and/or less than 250 μm in T89 temper, and/or less than 300 μm in T351 temper.

### Claim 61 (depends on 2)

An aluminum alloy rolled product according to claim 2, exhibiting in a corrosion test according to ASTM G 110 a maximum intergranular attack of less than 70 μm in T39 temper, and/or less than 180 μm in T851 temper, and/or less than 220 μm in T89 temper, and/or less than 270 μm in T351 temper.

### Claim 62 (depends on 3)

An aluminum alloy rolled product according to claim 3, exhibiting in a corrosion test according to ASTM G 110 a maximum intergranular attack of less than 70 μm in T39 temper, and/or less than 180 μm in T851 temper, and/or less than 220 μm in T89 temper, and/or less than 270 μm in T351 temper.

### Claim 63 (depends on 4)

An aluminum alloy rolled product according to claim 4, exhibiting in a corrosion test according to ASTM G 110 a maximum intergranular attack of less than 70 μm in T39 temper, and/or less than 180 μm in T851 temper, and/or less than 220 μm in T89 temper, and/or less than 270 μm in T351 temper.

### Claim 64 (depends on 5)

An aluminum alloy rolled product according to claim 5, exhibiting in a corrosion test according to ASTM G 110 a maximum intergranular attack of less than 70 μm in T39 temper, and/or less than 180 μm in T851 temper, and/or less than 220 μm in T89 temper, and/or less than 270 μm in T351 temper.

### Claim 65 (depends on 6)

An aluminum alloy rolled product according to claim 6, exhibiting in a corrosion test according to ASTM G 110 a maximum intergranular attack of less than 70 μm in T39 temper, and/or less than 180 μm in T851 temper, and/or less than 220 μm in T89 temper, and/or less than 270 μm in T351 temper.

### Claim 66 (depends on 7)

An aluminum alloy rolled product according to claim 7, exhibiting in a corrosion test according to ASTM G 110 a maximum intergranular attack of less than 70 μm in T39 temper, and/or less than 180 μm in T851 temper, and/or less than 220 μm in T89 temper, and/or less than 270 μm in T351 temper.

### Claim 67 (depends on 8)

An aluminum alloy rolled product according to claim 8, exhibiting in a corrosion test according to ASTM G 110 a maximum intergranular attack of less than 70 μm in T39 temper, and/or less than 180 μm in T851 temper, and/or less than 220 μm in T89 temper, and/or less than 270 μm in T351 temper.

### Claim 68 (depends on 9)

An aluminum alloy rolled product according to claim 9, exhibiting in a corrosion test according to ASTM G 110 a maximum intergranular attack of less than 70 μm in T39 temper, and/or less than 180 μm in T851 temper, and/or less than 220 μm in T89 temper, and/or less than 270 μm in T351 temper.

### Claim 69 (depends on 10)

An aluminum alloy rolled product according to claim 10, exhibiting in a corrosion test according to ASTM G 110 a maximum intergranular attack of less than 70 μm in T39 temper, and/or less than 180 μm in T851 temper, and/or less than 220 μm in T89 temper, and/or less than 270 μm in T351 temper.

### Claim 70 (depends on 11)

An aluminum alloy rolled product according to claim 11, exhibiting in a corrosion test according to ASTM G 110 a maximum intergranular attack of less than 70 μm in T39 temper, and/or less than 180 μm in T851 temper, and/or less than 220 μm in T89 temper, and/or less than 270 μm in T351 temper.

### Claim 71 (depends on 2)

A lower wing skin structural member made in an aluminum alloy rolled plate product according to claim 2.

### Claim 72 (depends on 3)

A lower wing skin structural member made in an aluminum alloy rolled plate product according to claim 3.

### Claim 73 (depends on 4)

A lower wing skin structural member made in an aluminum alloy rolled plate product according to claim 4.

### Claim 74 (depends on 5)

A lower wing skin structural member made in an aluminum alloy rolled plate product according to claim 5.

### Claim 75 (depends on 6)

A lower wing skin structural member made in an aluminum alloy rolled plate product according to claim 6.

### Claim 76 (depends on 7)

A lower wing skin structural member made in an aluminum alloy rolled plate product according to claim 7.

### Claim 77 (depends on 8)

A lower wing skin structural member made in an aluminum alloy rolled plate product according to claim 8.

### Claim 78 (depends on 9)

A lower wing skin structural member made in an aluminum alloy rolled plate product according to claim 9.

### Claim 79 (depends on 10)

A lower wing skin structural member made in an aluminum alloy rolled plate product according to claim 10.

### Claim 80 (depends on 11)

A lower wing skin structural member made in an aluminum alloy rolled plate product according to claim 11.

### Claim 81 (depends on 12)

A lower wing skin structural member made in an aluminum alloy rolled plate product according to claim 12.

### Claim 82 (depends on 2)

A fuselage skin member made in an aluminum alloy rolled plate or sheet product according to claim 2.

### Claim 83 (depends on 3)

A fuselage skin member made in an aluminum alloy rolled plate or sheet product according to claim 3.

### Claim 84 (depends on 4)

A fuselage skin member made in an aluminum alloy rolled plate or sheet product according to claim 4.

### Claim 85 (depends on 5)

A fuselage skin member made in an aluminum alloy rolled plate or sheet product according to claim 5.

### Claim 86 (depends on 6)

A fuselage skin member made in an aluminum alloy rolled plate or sheet product according to claim 6.

### Claim 87 (depends on 7)

A fuselage skin member made in an aluminum alloy rolled plate or sheet product according to claim 7.

### Claim 88 (depends on 8)

A fuselage skin member made in an aluminum alloy rolled plate or sheet product according to claim 8.

### Claim 89 (depends on 9)

A fuselage skin member made in an aluminum alloy rolled plate or sheet product according to claim 9.

### Claim 90 (depends on 10)

A fuselage skin member made in an aluminum alloy rolled plate or sheet product according to claim 10.

### Claim 91 (depends on 11)

A fuselage skin member made in an aluminum alloy rolled plate or sheet product according to claim 11.

### Claim 92 (depends on 12)

A fuselage skin member made in an aluminum alloy rolled plate or sheet product according to claim 12.

### Claim 93 (depends on 2)

A method for obtaining an aluminum alloy rolled product according to claim 2, wherein said rolled product comprises a plate, said method comprising:
Casting a rolling ingot, followed by optional stress relieving ,and scalping,
Homogenizing at a temperature between 450 and 510° C.,
Hot-rolling on a reversing mill, preferably with an exit temperature between 350 and 390° C.,
Optionally, for plate with a thickness of less than about 30 mm, conducting at least one intermediate reheating to about 480° C., followed by one or more hot-rolling passes, the final exit temperature optionally being between 350 and 370° C.,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching and natural aging,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 94 (depends on 3)

A method for obtaining an aluminum alloy rolled product according to claim 3, wherein said rolled product comprises a plate, said method comprising:
Casting a rolling ingot, followed by optional stress relieving ,and scalping,
Homogenizing at a temperature between 450 and 510° C.,
Hot-rolling on a reversing mill, preferably with an exit temperature between 350 and 390° C.,
Optionally, for plate with a thickness of less than about 30 mm, conducting at least one intermediate reheating to about 480° C., followed by one or more hot-rolling passes, the final exit temperature optionally being between 350 and 370° C.,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching and natural aging,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 95 (depends on 4)

A method for obtaining an aluminum alloy rolled product according to claim 4, wherein said rolled product comprises a plate, said method comprising:
Casting a rolling ingot, followed by optional stress relieving ,and scalping,
Homogenizing at a temperature between 450 and 510° C.,
Hot-rolling on a reversing mill, preferably with an exit temperature between 350 and 390° C.,
Optionally, for plate with a thickness of less than about 30 mm, conducting at least one intermediate reheating to about 480° C., followed by one or more hot-rolling passes, the final exit temperature optionally being between 350 and 370° C., Solution heat treating at a temperature between 490 and 510° C., followed by water quenching and natural aging,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 96 (depends on 5)

A method for obtaining an aluminum alloy rolled product according to claim 5, wherein said rolled product comprises a plate, said method comprising:
Casting a rolling ingot, followed by optional stress relieving ,and scalping,
Homogenizing at a temperature between 450 and 510° C.,
Hot-rolling on a reversing mill, preferably with an exit temperature between 350 and 390° C.,
Optionally, for plate with a thickness of less than about 30 mm, conducting at least one intermediate reheating to about 480° C., followed by one or more hot-rolling passes, the final exit temperature optionally being between 350 and 370° C.,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching and natural aging,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 97 (depends on 6)

A method for obtaining an aluminum alloy rolled product according to claim 6, wherein said rolled product comprises a plate, said method comprising:
Casting a rolling ingot, followed by optional stress relieving ,and scalping,
Homogenizing at a temperature between 450 and 510° C.,
Hot-rolling on a reversing mill, preferably with an exit temperature between 350 and 390° C.,
Optionally, for plate with a thickness of less than about 30 mm, conducting at least one intermediate reheating to about 480° C., followed by one or more hot-rolling passes, the final exit temperature optionally being between 350 and 370° C.,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching and natural aging,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 98 (depends on 7)

A method for obtaining an aluminum alloy rolled product according to claim 7, wherein said rolled product comprises a plate, said method comprising:
Casting a rolling ingot, followed by optional stress relieving ,and scalping,
Homogenizing at a temperature between 450 and 510° C.,
Hot-rolling on a reversing mill, preferably with an exit temperature between 350 and 390° C.,
Optionally, for plate with a thickness of less than about 30 mm, conducting at least one intermediate reheating to about 480° C., followed by one or more hot-rolling passes, the final exit temperature optionally being between 350 and 370° C.,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching and natural aging,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 99 (depends on 8)

A method for obtaining an aluminum alloy rolled product according to claim 8, wherein said rolled product comprises a plate, said method comprising:
Casting a rolling ingot, followed by optional stress relieving ,and scalping,
Homogenizing at a temperature between 450 and 510° C.,
Hot-rolling on a reversing mill, preferably with an exit temperature between 350 and 390° C.,
Optionally, for plate with a thickness of less than about 30 mm, conducting at least one intermediate reheating to about 480° C., followed by one or more hot-rolling passes, the final exit temperature optionally being between 350 and 370° C.,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching and natural aging,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 100 (depends on 9)

A method for obtaining an aluminum alloy rolled product according to claim 9, wherein said rolled product comprises a plate, said method comprising:
Casting a rolling ingot, followed by optional stress relieving ,and scalping,
Homogenizing at a temperature between 450 and 510° C.,
Hot-rolling on a reversing mill, preferably with an exit temperature between 350 and 390° C.,
Optionally, for plate with a thickness of less than about 30 mm, conducting at least one intermediate reheating to about 480° C., followed by one or more hot-rolling passes, the final exit temperature optionally being between 350 and 370° C.,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching and natural aging,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 101 (depends on 10)

A method for obtaining an aluminum alloy rolled product according to claim 10, wherein said rolled product comprises a plate, said method comprising:
Casting a rolling ingot, followed by optional stress relieving ,and scalping,
Homogenizing at a temperature between 450 and 510° C.,
Hot-rolling on a reversing mill, preferably with an exit temperature between 350 and 390° C.,
Optionally, for plate with a thickness of less than about 30 mm, conducting at least one intermediate reheating to about 480° C., followed by one or more hot-rolling passes, the final exit temperature optionally being between 350 and 370° C.,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching and natural aging,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 102

A method for obtaining an aluminum alloy rolled product according to claim11, wherein said rolled product comprises a plate, said method comprising:
Casting a rolling ingot, followed by optional stress relieving, and scalping,
Homogenizing at a temperature between 450 and 510° C.,
Hot-rolling on a reversing mill, preferably with an exit temperature between 350 and 390° C.,
Optionally, for plate with a thickness of less than about 30 mm, conducting at least one intermediate reheating to about 480° C., followed by one or more hot-rolling passes, the final exit temperature optionally being between 350 and 370° C.,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching and natural aging,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 103 (depends on 12)

A method for obtaining an aluminum alloy rolled product according to claim 12, wherein said rolled product comprises a plate, said method comprising:
Casting a rolling ingot, followed by optional stress relieving, and scalping,
Homogenizing at a temperature between 450 and 510° C.,
Hot-rolling on a reversing mill, preferably with an exit temperature between 350 and 390° C.,
Optionally, for plate with a thickness of less than about 30 mm, conducting at least one intermediate reheating to about 480° C., followed by one or more hot-rolling passes, the final exit temperature optionally being between 350 and 370° C.,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching and natural aging,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 104

A method for obtaining an aluminum alloy rolled product according to claim13, wherein said rolled product comprises a plate, said method comprising:
Casting a rolling ingot, followed by optional stress relieving, and scalping,
Homogenizing at a temperature between 450 and 510° C.,
Hot-rolling on a reversing mill, preferably with an exit temperature between 350 and 390° C.,
Optionally, for plate with a thickness of less than about 30 mm, conducting at least one intermediate reheating to about 480° C., followed by one or more hot-rolling passes, the final exit temperature optionally being between 350 and 370° C.,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching and natural aging,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 105 (depends on 14)

A method for obtaining an aluminum alloy rolled product according to claim 14, wherein said rolled product comprises a plate, said method comprising:
Casting a rolling ingot, followed by optional stress relieving, and scalping,
Homogenizing at a temperature between 450 and 510° C.,
Hot-rolling on a reversing mill, preferably with an exit temperature between 350 and 390° C.,
Optionally, for plate with a thickness of less than about 30 mm, conducting at least one intermediate reheating to about 480° C., followed by one or more hot-rolling passes, the final exit temperature optionally being between 350 and 370° C.,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching and natural aging,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 106

An aluminum alloy wherein when employed as plate or sheet, presents a compromise between fracture toughness and mechanical strength in that it is suitable for use in lower wingskin as well as fuselage products,
wherein when used as a sheet or thin plate fulfilling at least one of the following conditions (i) a tensile yield strength in the longitudinal direction (TYS(L)) of more than 400 MPa, and an apparent fracture toughness Kapp(T-L) of more than 110 MPa{square root}m, measured according to ASTM E 561 in the T-L orientation on a specimen with a width of W=127 mm; (ii) an ultimate tensile strength in the longitudinal direction (UTS(L)) of more than 450 MPa, and an elongation at fracture in the longitudinal direction of more than 24%; and/or (iii) a tensile yield strength in the longitudinal direction (TYS(L)) of more than 400 MPa, and a Kahn stress Re of at least 180 MPa,,
and further wherein, when employed as thick plate having at least one the following combinations of properties : (i) a UTS(L) of more than 500 MPa, and a Kapp(L-T) of more than 75 MPa{square root}m, measured according to ASTM E 561 on a 6.35 mm thick C(T) specimen with a width of W=40 mm; (ii) a tensile yield strength in the longitudinal direction (TYS(L)) of more than 450 MPa and a Kapp(L-T) of more than 77 MPa{square root}m, measured according to ASTM E 561 on a 6.35 mm thick C(T) specimen with a width of W=40 mm; and/or (iii) a tensile yield strength in the longitudinal direction (TYS(L)) of more than 350 MPa and a Kahn stress Re of at least 190 MPa.

### Claim 107 (depends on 2)

A method for obtaining a rolled product according to claim 2 comprising a sheet product, said method comprising:
Casting a rolling ingot, followed by optional stress relieving, and scalping,
Homogenizing at a temperature between 470 and 530° C.,
Hot-rolling down to a thickness of less than 12 mm, and not more than 200% of final thickness, with a final exit temperature between 230 and 350° C.,
Optionally cold rolling,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 108 (depends on 3)

A method for obtaining a rolled product according to claim 3 comprising a sheet product, said method comprising:
Casting a rolling ingot, followed by optional stress relieving, and scalping,
Homogenizing at a temperature between 470 and 530° C.,
Hot-rolling down to a thickness of less than 12 mm, and not more than 200% of final thickness, with a final exit temperature between 230 and 350° C.,
Optionally cold rolling,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 109 (depends on 4)

A method for obtaining a rolled product according to claim 4 comprising a sheet product, said method comprising:
Casting a rolling ingot, followed by optional stress relieving, and scalping,
Homogenizing at a temperature between 470 and 530° C.,
Hot-rolling down to a thickness of less than 12 mm, and not more than 200% of final thickness, with a final exit temperature between 230 and 350° C.,
Optionally cold rolling,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 110 (depends on 5)

A method for obtaining a rolled product according to claim 5 comprising a sheet product, said method comprising:
Casting a rolling ingot, followed by optional stress relieving, and scalping,
Homogenizing at a temperature between 470 and 530° C.,
Hot-rolling down to a thickness of less than 12 mm, and not more than 200% of final thickness, with a final exit temperature between 230 and 350° C.,
Optionally cold rolling,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 111 (depends on 6)

A method for obtaining a rolled product according to claim 6 comprising a sheet product, said method comprising:
Casting a rolling ingot, followed by optional stress relieving, and scalping,
Homogenizing at a temperature between 470 and 530° C.,
Hot-rolling down to a thickness of less than 12 mm, and not more than 200% of final thickness, with a final exit temperature between 230 and 350° C.,
Optionally cold rolling,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 112 (depends on 7)

A method for obtaining a rolled product according to claim 7 comprising a sheet product, said method comprising:
Casting a rolling ingot, followed by optional stress relieving, and scalping,
Homogenizing at a temperature between 470 and 530° C.,
Hot-rolling down to a thickness of less than 12 mm, and not more than 200% of final thickness, with a final exit temperature between 230 and 350° C.,
Optionally cold rolling,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 113 (depends on 8)

A method for obtaining a rolled product according to claim 8 comprising a sheet product, said method comprising:
Casting a rolling ingot, followed by optional stress relieving, and scalping,
Homogenizing at a temperature between 470 and 530° C.,
Hot-rolling down to a thickness of less than 12 mm, and not more than 200% of final thickness, with a final exit temperature between 230 and 350° C.,
Optionally cold rolling,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 114 (depends on 9)

A method for obtaining a rolled product according to claim 9 comprising a sheet product, said method comprising:
Casting a rolling ingot, followed by optional stress relieving, and scalping,
Homogenizing at a temperature between 470 and 530° C.,
Hot-rolling down to a thickness of less than 12 mm, and not more than 200% of final thickness, with a final exit temperature between 230 and 350° C.,
Optionally cold rolling,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 115 (depends on 10)

A method for obtaining a rolled product according to claim 10 comprising a sheet product, said method comprising:
Casting a rolling ingot, followed by optional stress relieving, and scalping,
Homogenizing at a temperature between 470 and 530° C.,
Hot-rolling down to a thickness of less than 12 mm, and not more than 200% of final thickness, with a final exit temperature between 230 and 350° C.,
Optionally cold rolling,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 116 (depends on 11)

A method for obtaining a rolled product according to claim 11 comprising a sheet product, said method comprising:
Casting a rolling ingot, followed by optional stress relieving, and scalping,
Homogenizing at a temperature between 470 and 530° C.,
Hot-rolling down to a thickness of less than 12 mm, and not more than 200% of final thickness, with a final exit temperature between 230 and 350° C.,
Optionally cold rolling,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 117 (depends on 12)

A method for obtaining a rolled product according to claim 12 comprising a sheet product, said method comprising:
Casting a rolling ingot, followed by optional stress relieving, and scalping,
Homogenizing at a temperature between 470 and 530° C.,
Hot-rolling down to a thickness of less than 12 mm, and not more than 200% of final thickness, with a final exit temperature between 230 and 350° C.,
Optionally cold rolling,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 118 (depends on 13)

A method for obtaining a rolled product according to claim 13 comprising a sheet product, said method comprising:
Casting a rolling ingot, followed by optional stress relieving, and scalping,
Homogenizing at a temperature between 470 and 530° C.,
Hot-rolling down to a thickness of less than 12 mm, and not more than 200% of final thickness, with a final exit temperature between 230 and 350° C.,
Optionally cold rolling,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.

### Claim 119 (depends on 14)

A method for obtaining a rolled product according to claim 14 comprising a sheet product, said method comprising:
Casting a rolling ingot, followed by optional stress relieving, and scalping,
Homogenizing at a temperature between 470 and 530° C.,
Hot-rolling down to a thickness of less than 12 mm, and not more than 200% of final thickness, with a final exit temperature between 230 and 350° C.,
Optionally cold rolling,
Solution heat treating at a temperature between 490 and 510° C., followed by water quenching,
Cold working by stretching alone or cold rolling followed by stretching, optionally followed by artificial aging.