# US 2004/0079449 A1 · Iron base rare earth alloy powder and compound comprising iron base rare earth alloy powder and permanent magnet using the same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2004/0079449 A1
- Document ID: US20040079449A1
- Status: Published application
- Kind: A1
- Application number: 10/470,547
- Filed: 2003-07-30
- Published: 2004-04-29
- Earliest claimed: 2001-02-07
- Assignees: Neomax Co., Ltd.
- Inventors: Hirokazu Kanekiyo; Hirokazu Kitayama; Satoshi Hirosawa; Toshio Miyoshi
- Web page: https://patentgrep.com/patent/US20040079449A1

## CPC

- B22F 3/225: {by injection molding}
- B22F 7/08: with one or more parts not made from powder {(B22F7/062 takes precedence)}
- C22C 33/0207: {Using a mixture of pre-alloyed powders or a master alloy}
- H01F 1/0571: {in the form of particles, e.g. rapid quenched powders or ribbon flakes}
- H01F 1/0578: {bonded together}
- H01F 1/058: and IVa elements, e.g. Gd2Fe14C
- B22F 2998/00: Supplementary information concerning processes or compositions relating to powder metallurgy
- B22F 2998/10: Processes characterised by the sequence of their steps
- B22F 2999/00: Aspects linked to processes or compositions used in powder metallurgy
- B22F: WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER (making alloys by powder metallurgy C22C); APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- H01F: MAGNETS; INDUCTANCES; TRANSFORMERS; SELECTION OF MATERIALS FOR THEIR MAGNETIC PROPERTIES

## Abstract

An iron-based rare-earth alloy powder includes: a first iron-based rare-earth alloy powder, which has a mean particle size of 10 μm to 70 μm and of which the powder particles have aspect ratios of 0.4 to 1.0; and a second iron-based rare-earth alloy powder, which has a mean particle size of 70 μm to 300 μm and of which the powder particles have aspect ratios of less than 0.3. The first and second iron-based rare-earth alloy powders are mixed at a volume ratio of 1:49 to 4:1. In this manner, an iron-based rare-earth alloy powder with increased flowability and a compound to make a magnet are provided.

## Claims

### Claim 1

An iron-based rare-earth alloy powder comprising:
a first iron-based rare-earth alloy powder, which has a mean particle size of 10 μm to 70 μm and of which the powder particles have aspect ratios of 0.4 to 1.0; and
a second iron-based rare-earth alloy powder, which has a mean particle size of 70 μm to 300 μm and of which the powder particles have aspect ratios of less than 0.3,
wherein the first and second iron-based rare-earth alloy powders are mixed at a volume ratio of 1:49 to 4:1.

### Claim 2 (depends on 1)

The iron-based rare-earth alloy powder of claim 1, wherein the first iron-based rare-earth alloy powder has a composition represented by the general formula:
(Fe1-mTm)100-x-y-zQxRyMz
where T is at least one element selected from the group consisting of Co and Ni; Q is at least one element selected from the group consisting of B and C and always includes B; R is at least one rare-earth element selected from the group consisting of Pr, Nd, Dy and Tb; M is at least one element selected from the group consisting of Al, Si, Ti, V, Cr, Mn, Cu, Zn, Ga, Zr, Nb, Mo, Ag, Hf, Ta, W, Pt, Au and Pb; and the mole fractions x, y, and z satisfy the inequalities of: 10 at %≦x≦30 at %; 2 at %≦y<10 at %; 0 at %≦z≦10 at %; and 0≦m≦0.5, respectively.

### Claim 3 (depends on 2)

The iron-based rare-earth alloy powder of claim 2, wherein the first iron-based rare-earth alloy powder includes, as its constituent phases, an Fe phase, an FeB compound phase and a compound phase having an R2Fe14B-type crystalline structure, and the respective constituent phases have an average crystal grain size of 150 nm or less.

### Claim 4 (depends on 1)

The iron-based rare-earth alloy powder of claim 1, wherein the first iron-based rare-earth alloy powder has a composition represented by the general formula:
(Fe1-mTm)100-x-y-zQxRyMz
where T is at least one element selected from the group consisting of Co and Ni; Q is at least one element selected from the group consisting of B and C and always includes B; R is at least one rare-earth element selected from the group consisting of Pr, Nd, Dy and Tb; M is at least one element selected from the group consisting of Al, Si, Ti, V, Cr, Mn, Cu, Zn, Ga, Zr, Nb, Mo, Ag, Hf, Ta, W, Pt, Au and Pb and always includes Ti; and the mole fractions x, y, z and m satisfy the inequalities of: 10 at %<x≦20 at %; 6 at %<y<10 at %; 0.1 at %≦z≦12 at %; and 0≦m≦0.5, respectively.

### Claim 5 (depends on 4)

The iron-based rare-earth alloy powder of claim 4, wherein the first iron-based rare-earth alloy powder includes at least two ferromagnetic crystalline phases, of which hard magnetic phases have an average crystal grain size of 5 nm to 200 nm and soft magnetic phases have an average crystal grain size of 1 nm to 100 nm.

### Claim 6 (depends on 1, 2, 3, 4, 5)

The iron-based rare-earth alloy powder of one of claims 1 to 5, wherein the second iron-based rare-earth alloy powder has a composition represented by the general formula:
Fe100-x-yQxRy
where Fe is iron; Q is at least one element selected from the group consisting of B and C and always includes B; R is at least one rare-earth element selected from the group consisting of Pr, Nd, Dy and Tb; and the mole fractions x and y satisfy the inequalities of 1 at %≦x≦6 at % and 10 at %≦y≦25 at %, respectively.

### Claim 7 (depends on 1, 2, 3, 4, 5, 6)

A compound for use to make a magnet, the compound comprising the iron-based rare-earth alloy powder of one of claims 1 to 6 and a resin.

### Claim 8 (depends on 7)

The compound of claim 7, wherein the resin is a thermoplastic resin.

### Claim 9 (depends on 7, 8)

A permanent magnet, made of the compound of claim 7 or 8.

### Claim 10 (depends on 9)

The permanent magnet of claim 9, wherein the permanent magnet has a density of at least 4.5 g/cm3.

### Claim 11 (depends on 9, 10)

A motor comprising:
a rotor including the permanent magnet of claim 9 or 10; and
a stator, which is provided so as to surround the rotor.

### Claim 12

A method of making an iron-based rare-earth alloy powder, the method comprising the steps of:
(a) providing a first iron-based rare-earth alloy powder, which has a mean particle size of 10 μm to 70 μm and of which the powder particles have aspect ratios of 0.4 to 1.0;
(b) providing a second iron-based rare-earth alloy powder, which has a mean particle size of 70 μm to 300 μm and of which the powder particles have aspect ratios of less than 0.3; and
(c) mixing the first and second iron-based rare-earth alloy powders at a volume ratio of 1:49 to 4:1.

### Claim 13 (depends on 12)

The method of claim 12, wherein the first iron-based rare-earth alloy powder has a composition represented by the general formula:
(Fe1-mTm)100-x-y-zQxRyMz
where T is at least one element selected from the group consisting of Co and Ni; Q is at least one element selected from the group consisting of B and C and always includes B; R is at least one rare-earth element selected from the group consisting of Pr, Nd, Dy and Tb; M is at least one element selected from the group consisting of Al, Si, Ti, V, Cr, Mn, Cu, Zn, Ga, Zr, Nb, Mo, Ag, Hf, Ta, W, Pt, Au and Pb; and the mole fractions x, y, and z satisfy the inequalities of: 10 at %≦x≦30 at %; 2 at %≦y≦10 at %; 0 at %≦z≦10 at %; and 0≦m≦0.5, respectively.

### Claim 14 (depends on 12)

The method of claim 12, wherein the first iron-based rare-earth alloy powder has a composition represented by the general formula:
(Fe1-mTm)100-x-y-zQxRyMz
where T is at least one element selected from the group consisting of Co and Ni; Q is at least one element selected from the group consisting of B and C and always includes B; R is at least one rare-earth element selected from the group consisting of Pr, Nd, Dy and Tb; M is at least one element selected from the group consisting of Al, Si, Ti, V, Cr, Mn, Cu, Zn, Ga, Zr, Nb, Mo, Ag, Hf, Ta, W, Pt, Au and Pb and always includes Ti; and the mole fractions x, y, z and m satisfy the inequalities of: 10 at %<x≦20 at %; 6 at %<y<10 at %; 0.1 at %≦z≦12 at %; and 0≦m≦0.5, respectively.

### Claim 15 (depends on 12, 13, 14)

The method of one of claims 12 to 14, wherein the step (a) includes the steps of:
cooling a melt of the first iron-based rare-earth alloy by a melt-quenching process, thereby forming a rapidly solidified alloy with a thickness of 70 μm to 300 μm; and
pulverizing the rapidly solidified alloy.

### Claim 16 (depends on 15)

The method of claim 15, further comprising the step of thermally treating and crystallizing the rapidly solidified alloy before the step of pulverizing is performed.

### Claim 17 (depends on 15, 16)

The method of claim 15 or 16, wherein the step of pulverizing is carried out with a pin mill machine or a hammer mill machine.

### Claim 18 (depends on 15, 16, 17)

The method of one of claims 15 to 17, wherein the rapidly solidified alloy includes at least one metastable phase, which is selected from the group consisting of Fe23B6, Fe3B, R2Fe14B and R2Fe23B phases, and/or an amorphous phase.

### Claim 19 (depends on 15, 16, 17, 18)

The method of one of claims 15 to 18, wherein the step of cooling includes the step of bringing the melt into contact with a roller, which is rotating at a roller surface peripheral velocity of 1 m/s to 13 m/s, thereby forming the rapidly solidified alloy.

### Claim 20 (depends on 19)

The method of claim 19, wherein the step of cooling is carried out within a reduced-pressure atmosphere.

### Claim 21 (depends on 20)

The method of claim 20, wherein the reduced-pressure atmosphere has an absolute pressure of 1.3 kPa to 90 kPa.

### Claim 22 (depends on 12, 13, 14, 15, 16, 17, 18, 19, 20, 21)

The method of one of claims 12 to 21, wherein the second iron-based rare-earth alloy powder has a composition represented by the general formula:
Fe100-x-yQxRy
where Fe is iron; Q is at least one element selected from the group consisting of B and C and always includes B; R is at least one rare-earth element selected from the group consisting of Pr, Nd, Dy and Tb; and the mole fractions x and y satisfy the inequalities of 1 at %≦x≦6 at % and 10 at %≦y≦25 at %, respectively.

### Claim 23 (depends on 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22)

A method of making a compound for use to make a magnet, the method comprising the steps of:
preparing the iron-based rare-earth alloy powder by the method of one of claims 12 to 22; and
mixing the iron-based rare-earth alloy powder and a resin together.

### Claim 24 (depends on 23)

The method of claim 23, wherein the resin is a thermoplastic resin.

### Claim 25 (depends on 24)

A method for producing a permanent magnet comprising the step of injection-molding the compound made by the method of claim 24.

### Claim 26 (depends on 24)

A method for fabricating a motor, comprising the steps of:
preparing a rotor, which has a magnet slot in its iron core;
injection-molding the compound for use to make a magnet, made by the method of claim 24, in the magnet slot; and
providing a stator that surrounds the rotor.