# US 2004/0079446 A1 · Magnetic alloy material and method of making the magnetic alloy material

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2004/0079446 A1
- Document ID: US20040079446A1
- Status: Published application
- Kind: A1
- Application number: 10/642,276
- Filed: 2003-08-18
- Published: 2004-04-29
- Earliest claimed: 2002-08-21
- Assignees: Neomax Co., Ltd.
- Inventors: Ryosuke Kogure; Hirokazu Kanekiyo; Takeshi Nishiuchi; Satoshi Hirosawa
- Web page: https://patentgrep.com/patent/US20040079446A1

## CPC

- H01F 1/015: {Metals or alloys}
- H01F 1/0571: {in the form of particles, e.g. rapid quenched powders or ribbon flakes}
- H01F: MAGNETS; INDUCTANCES; TRANSFORMERS; SELECTION OF MATERIALS FOR THEIR MAGNETIC PROPERTIES

## Abstract

A method of making a magnetic alloy material includes the steps of: preparing a melt of an alloy material having a predetermined composition; rapidly cooling and solidifying the melt to obtain a rapidly solidified alloy represented by: Fe100-a-b-cREaAbTMc where RE is at least one rare-earth element selected from La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er and Tm and including at least about 90 at % of La; A is at least one element selected from Al, Si, Ga, Ge and Sn; TM is at least one transition metal element selected from Sc, Ti, V, Cr, Mn, Co, Ni, Cu and Zn; and 5 at %≦a≦10 at %, 4.7 at %≦b≦18 at % and 0 at %≦c≦9 at %; and producing a compound phase having an NaZn13-type crystal structure in at least about 70 vol % of the rapidly solidified alloy.

## Claims

### Claim 1

A method of making a magnetic alloy material, the method comprising the steps of:
preparing a melt of an alloy material having a predetermined composition;
rapidly cooling and solidifying the melt of the alloy material to obtain a rapidly solidified alloy having a composition represented by the general formula:
Fe100-a-b-cREaAbTMc
where RE is at least one rare-earth element that is selected from the group consisting of La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er and Tm and that includes at least about 90 at % of La; A is at least one element that is selected from the group consisting of Al, Si, Ga, Ge and Sn; TM is at least one transition metal element that is selected from the group consisting of Sc, Ti, V, Cr, Mn, Co, Ni, Cu and Zn; and mole fractions a, b and c satisfy 5 at %≦a≦10 at %, 4.7 at %≦b≦18 at % and 0 at %≦c≦9 at %, respectively; and
producing a compound phase having an NaZn13-type crystal structure in at least about 70 vol % of the rapidly solidified alloy.

### Claim 2 (depends on 1)

The method of claim 1, wherein the step of producing the compound phase includes the step of thermally treating the rapidly solidified alloy at a temperature of about 400° C. to about 1,200° C. for a period of time of about 1 second to about 100 hours.

### Claim 3 (depends on 2)

The method of claim 2, wherein the step of thermally treating includes the step of thermally treating the rapidly solidified alloy for at least about 10 minutes.

### Claim 4 (depends on 2)

The method of claim 2, wherein the step of thermally treating includes the step of producing a homogeneous NaZn13-type crystal structure in the overall rapidly solidified alloy.

### Claim 5 (depends on 1)

The method of claim 1, wherein the step of rapidly cooling and solidifying the melt immediately produces the compound phase having the NaZn13-type crystal structure.

### Claim 6 (depends on 1)

The method of claim 1, wherein the step of rapidly cooling and solidifying the melt includes the step of rapidly cooling and solidifying the melt at a cooling rate of about 1×102° C./s to about 1×108° C./s.

### Claim 7 (depends on 1)

The method of claim 1, wherein the step of rapidly cooling and solidifying the melt produces a thin-strip rapidly solidified alloy having a thickness of about 10 μm to about 300 μm.

### Claim 8 (depends on 1)

The method of claim 1, wherein the magnetic alloy material exhibits a magnetocaloric effect.

### Claim 9 (depends on 1)

The method of claim 1, further comprising the step of pulverizing the rapidly solidified alloy.

### Claim 10 (depends on 1)

The method of claim 1, wherein the magnetic alloy material has a Curie temperature Tc of about 180 K to about 330 K to represent a magnetic phase transition.

### Claim 11 (depends on 1)

The method of claim 1, wherein the step of rapidly cooling and solidifying the melt includes the step of obtaining a rapidly solidified alloy including Co as TM.

### Claim 12 (depends on 1)

The method of claim 1, wherein a temperature range in which the magnetic phase transition occurs has a half width ΔTc of at least about 30 K.

### Claim 13

A magnetic alloy material made by a method comprising the steps of:
preparing a melt of an alloy material having a predetermined composition;
rapidly cooling and solidifying the melt of the alloy material to obtain a rapidly solidified alloy having a composition represented by the general formula:
Fe100-a-b-cREaAbTMc
where RE is at least one rare-earth element that is selected from the group consisting of La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er and Tm and that includes at least about 90 at % of La; A is at least one element that is selected from the group consisting of Al, Si, Ga, Ge and Sn; TM is at least one transition metal element that is selected from the group consisting of Sc, Ti, V, Cr, Mn, Co, Ni, Cu and Zn; and mole fractions a, b and c satisfy 5 at %≦a≦10 at %, 4.7 at %≦b≦18 at % and 0 at %≦c≦9 at %, respectively; and
producing a compound phase having an NaZn13-type crystal structure in at least about 70 vol % of the rapidly solidified alloy.