# US 2004/0079445 A1 · High performance magnetic materials with low flux-aging loss

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2004/0079445 A1
- Document ID: US20040079445A1
- Status: Published application
- Kind: A1
- Application number: 10/278,843
- Filed: 2002-10-24
- Published: 2004-04-29
- Earliest claimed: 2002-10-24
- Inventors: Zhongmin Chen; Benjamin R. Smith; Bao-Min Ma
- Web page: https://patentgrep.com/patent/US20040079445A1

## CPC

- H01F 1/0578: {bonded together}
- H01F 1/0571: {in the form of particles, e.g. rapid quenched powders or ribbon flakes}
- H01F 41/0266: {Moulding; Pressing (H01F41/0273 takes precedence; hard magnetic particles H01F1/06, H01F1/11)}
- H01F: MAGNETS; INDUCTANCES; TRANSFORMERS; SELECTION OF MATERIALS FOR THEIR MAGNETIC PROPERTIES

## Abstract

The present invention relates to magnetic materials made by rapid solidification processes which exhibit high remanence and intrinsic coercivity values and low flux-aging loss. More specifically, the invention relates to isotropic Nd—Fe—B type materials with remanence and intrinsic coercivity values of greater than 8.0 kG and 10.0 kOe, respectively, at room temperature, and bonded magnets made from the magnetic materials with low flux-aging loss and are suitable for high temperature applications. The invention also relates to methods of making the magnetic materials and the bonded magnets.

## Claims

### Claim 1

A magnetic material having been prepared by a rapid solidification process, followed by a thermal annealing process at a temperature range of about 350° C. to about 700° C. for about 2 to about 120 minutes, said magnetic material having the composition, in atomic percentage, of
RExFe100-x-y-zMyBz
wherein RE is one or more of Y, La, Ce, Pr, Nd, Sm, Er, Gd, Tb, Dy, Ho, Tm, Yb and Lu; M is one or more of Nb, Ti, Cr, Mo, W, and Hf; x is from about 11.0 to about 12.5; y is from about 0.5 to about 3; and z is from about 4.5 to about 7.0; and
wherein the magnetic material exhibits a remanence (Br) value of greater than about 8.0 kG and an intrinsic coercivity (Hci) value of greater than about 10.0 kOe.

### Claim 2 (depends on 1)

The magnetic material of claim 1, wherein the rapid solidification process is a melt-spinning or jet-casting process.

### Claim 3 (depends on 1)

The magnetic material of claim 1, wherein RE is Nd.

### Claim 4 (depends on 1)

The magnetic material of claim 1, wherein M is Nb, Ti, or Cr.

### Claim 5 (depends on 4)

The magnetic material of claim 4, wherein M is Nb or Ti.

### Claim 6 (depends on 5)

The magnetic material of claim 5, wherein M is Nb.

### Claim 7 (depends on 1)

The magnetic material of claim 1, wherein x, y and z are independent from each and are from about 11.1 to about 12.0, from about 1.0 to about 2.0 and from about 5.0 to about 6.0, respectively.

### Claim 8 (depends on 7)

The magnetic material of claim 7, wherein x is from about 11.2 to about 11.9, y is from about 1.2 to about 1.8 and z is from about 5.3 to about 6.5.

### Claim 9 (depends on 8)

The magnetic material of claim 8, wherein x is from about 11.4 to about 11.7, y is from about 1.3 to about 1.7 and z is from about 5.7 to about 6.0.

### Claim 10 (depends on 1)

The magnetic material of claim 1, wherein the thermal annealing process is at a temperature range of about 600° C. to about 700° C. for about 2 to about 10 minutes.

### Claim 11 (depends on 1)

The magnetic material of claim 1, wherein the material exhibits a Br value of greater than about 8.3 kG and an Hci value of greater than about 12.0 kOe.

### Claim 12 (depends on 1)

The magnetic material of claim 1, wherein the material exhibits a near stoichiometric Nd2Fe14B single-phase microstructure, as determined by X-Ray diffraction.

### Claim 13 (depends on 1)

The magnetic material of claim 1, wherein the material has crystal grain sizes ranging from about 1 nm to about 50 nm.

### Claim 14 (depends on 13)

The magnetic material of claim 13, wherein the material has crystal grain sizes ranging from about 5 nm to about 20 nm.

### Claim 15

A bonded magnet comprising a bonding agent and a magnetic material, said magnetic material having been prepared by a rapid solidification process, followed by a thermal annealing process at a temperature range of about 350° C. to about 700° C. for about 2 to about 120 minutes, and having the composition, in atomic percentage, of
RExFe100-x-y-zMyBz
wherein RE is one or more of Y, La, Ce, Pr, Nd, Sm, Er, Gd, Tb, Dy, Ho, Tm, Yb and Lu; M is one or more of Nb, Ti, Cr, Mo, W, and Hf; x is from about 11.0 to about 12.5, y is from about 0.5 to about 3, and z is from about 4.5 to about 7.0; and
wherein the magnetic material exhibits a remanence (Br) value of greater than about 8.0 kG and an intrinsic coercivity (Hci) value of greater than about 10.0 kOe.

### Claim 16 (depends on 15)

The bonded magnet of claim 15, wherein the bonding agent is epoxy, polyamide, polyphenylene sulfide, a liquid crystalline polymer, or combinations thereof.

### Claim 17 (depends on 16)

The bonded magnet of claim 16, wherein the bonding agent is epoxy.

### Claim 18 (depends on 15)

The bonded magnet of claim 15, wherein the bonding agent further comprises one or more additives selected from a high molecular weight multi-functional fatty acid ester, stearic acid, hydroxy stearic acid, a high molecular weight comples ester, a long chain ester of pentaerythritol, palmitic acid, a polyethylene based lubricant concentrate, an ester of montanic acid, a partly saponified ester of montanic acid, a polyolefin wax, a fatty bis-amide, a fatty acid secondary amide, a polyoctanomer with high trans content, a maleic anhydride, a glycidyl-functional acrylic hardener, zinc stearate, and a polymeric plasticizer.

### Claim 19 (depends on 18)

The bonded magnet of claim 18, wherein the additive is zinc stearate.

### Claim 20 (depends on 15)

The bonded magnet of claim 15, wherein the magnet comprises, by weight, from about 1% to about 5% epoxy and from about 0.01% to about 0.05% zinc stearate.

### Claim 21 (depends on 20)

The bonded magnet of claim 20, wherein the magnet comprises, by weight, about 2% epoxy and about 0.02% zinc stearate.

### Claim 22 (depends on 15)

The bonded magnet of claim 15, wherein the magnet is made by compression molding, injection molding, calendering, extrusion, screen printing, or combinations thereof.

### Claim 23 (depends on 22)

The bonded magnet of claim 22, wherein the magnet has a permeance coefficient of from about 0.2 to about 12.0.

### Claim 24 (depends on 15)

The bonded magnet of claim 15, wherein the magnet exhibit a flux-aging loss of less than about 7.0% when aged at 180° C. for 100 hours.

### Claim 25 (depends on 24)

The bonded magnet of claim 24, wherein the magnet exhibit a flux-aging loss of less than about 6.0%.

### Claim 26 (depends on 25)

The bonded magnet of claim 25, wherein the magnet exhibit a flux-aging loss of less than about 5.5%.

### Claim 27

A method of making a magnetic material comprising
forming a melt comprising the composition, in atomic percentage, of
RExFe100-x-y-zMyBz;
rapidly solidifying the melt to obtain a magnetic powder;
thermally annealing the magnetic powder at a temperature range of about 350° C. to about 700° C. for about 2 to about 120 minutes;
wherein RE is one or more of Y, La, Ce, Pr, Nd, Sm, Er, Gd, Tb, Dy, Ho, Tm, Yb and Lu; M is one or more of Nb, Ti, Cr, Mo, W, and Hf; x is from about 11.0 to about 12.5; y is from about 0.5 to about 3; and z is from about 4.5 to about 7.0; and
wherein the magnetic material exhibits a remanence (Br) value of greater than about 8.0 kG and an intrinsic coercivity (Hci) value of greater than about 10.0 kOe.

### Claim 28

A method of making a bonded magnet comprising
forming a melt comprising the composition, in atomic percentage, of
RExFe100-x-y-zMyBz;
rapidly solidifying the melt to obtain a magnetic powder;
thermally annealing the powder at a temperature range of about 350° C. to about 700° C. for about 2 to about 120 minutes;
mixing and/or coating the magnetic powder with a binding agent; and
pressing and/or molding the powders and binding agent;
wherein RE is one or more of Y, La, Ce, Pr, Nd, Sm, Er, Gd, Tb, Dy, Ho, Tm, Yb and Lu; M is one or more of Nb, Ti, Cr, Mo, W, and Hf; x is from about 11.0 to about 12.5; y is from about 0.5 to about 3; and z is from about 4.5 to about 7.0; and
wherein the magnetic material exhibits a remanence (Br) value of greater than about 8.0 kG and an intrinsic coercivity (Hci) value of greater than about 10.0 kOe.