# US 2004/0072009 A1 · Copper sputtering targets and methods of forming copper sputtering targets

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2004/0072009 A1
- Document ID: US20040072009A1
- Status: Published application
- Kind: A1
- Application number: 10/614,807
- Filed: 2003-07-09
- Published: 2004-04-15
- Earliest claimed: 1999-12-16
- Inventors: Vladimir M. Segal; Wuwen Yi; Stephane Ferrasse; Chi Tse Wu; Susan D. Strothers; Frank A. Alford; William B. Willett
- Web page: https://patentgrep.com/patent/US20040072009A1

## CPC

- B21C 23/01: starting from material of particular form or shape, e.g. mechanically pre-treated (B21C23/22 takes precedence)
- B21C 23/001: {to improve the material properties, e.g. lateral extrusion}
- C22F 1/08: of copper or alloys based thereon
- C23C 14/3414: {Metallurgical or chemical aspects of target preparation, e.g. casting, powder metallurgy}
- Y10T 428/12118: Nonparticulate component has Ni-, Cu-, or Zn-base
- B21C: MANUFACTURE OF METAL SHEETS, WIRE, RODS, TUBES, PROFILES OR LIKE SEMI-MANUFACTURED PRODUCTS OTHERWISE THAN BY ROLLING; AUXILIARY OPERATIONS USED IN CONNECTION WITH METAL-WORKING WITHOUT ESSENTIALLY REMOVING MATERIAL
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- Y10T: TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION

## Abstract

The invention includes a copper-comprising sputtering target. The target is monolithic or bonded and contains at least 99.99% copper by weight and has an average grain size of from 1 micron to 50 microns. The copper-comprising target has a yield strength of greater than or equal to about 15 ksi and a Brinell hardness (HB) of greater than about 40. The invention includes copper alloy monolithic and bonded sputtering targets consisting essentially of less than or equal to about 99.99% copper by weight and a total amount of alloying element(s) of at least 100 ppm and less than 10% by weight. The targets have an average grain size of from less than 1 micron to 50 microns and have a grain size non-uniformity of less than about 15% standard deviation (1-sigma) throughout the target. The invention additionally includes methods of producing bonded and monolithic copper and copper alloy targets.

## Claims

### Claim 1

A copper-comprising sputtering target comprising:
at least 99.99 % copper, by weight;
an average grain size of from at least 1 micron to less than or equal to about 50 microns; and
the target having a yield strength of greater than or equal to about 15 ksi.

### Claim 2 (depends on 1)

The target of claim 1 wherein the target has a hardness of at least 40 HB.

### Claim 3 (depends on 1)

The target of claim 1 having an ultimate tensile strength at least 15% greater than a target having a substantially identical elemental composition with an average grain size of 50 microns.

### Claim 4 (depends on 1)

The sputtering target of claim 1 wherein the hardness is at least 15% greater than a target having a substantially identical elemental composition with an average grain size of 50 microns.

### Claim 5 (depends on 1)

The sputtering target of claim 1 wherein the yield strength is at least 10% greater than a target having a substantially identical elemental composition with an average grain size of 50 microns.

### Claim 6 (depends on 1)

The sputtering target of claim 1 wherein the target is monolithic and has a sputtering lifetime at least 30% longer than an alternative bonded target having a substantially identical elemental composition with an average grain size of 50 microns.

### Claim 7 (depends on 1)

The target of claim 1 wherein the target comprises at least 99.999% copper, by weight

### Claim 8 (depends on 1)

The target of claim 1 wherein the target comprises at least 99.9999% copper, by weight.

### Claim 9 (depends on 1)

The target of claim 1 wherein the target comprises at least 99.9995% copper, by weight.

### Claim 10 (depends on 1)

The target of claim 1 wherein the target comprises a grain size uniformity having a non-uniformity of less than or equal to 20%.

### Claim 11 (depends on 10)

The target of claim 10 wherein the non-uniformity is less than 15% (1-sigma).

### Claim 12 (depends on 1)

The target of claim 1 wherein the-target comprises a grain size uniformity having a standard deviation of less than or equal to 10% (1-sigma).

### Claim 13 (depends on 1)

The target of claim 1 wherein the target is diffusion bonded to a backing plate, the diffusion bond having a bond yield strength of greater than 10 ksi.

### Claim 14 (depends on 13)

The target of claim 13 wherein the bond yield strength is greater than or equal to about 15 ksi.

### Claim 15 (depends on 1)

The target of claim 1 wherein the average grain size is from about 5 microns to about 20 microns.

### Claim 16

A copper alloy sputtering target consisting essentially of:
less than or equal to about 99.99% copper, by weight;
at least one alloying element selected from the group consisting of Cd, Ca, Au, Ag, Be, Li, Mg, Al, Pd, Hg, Ni, In, Zn, B, Ga, Mn, Sn, Ge, W, Cr, O, Sb, Ir, P, As, Co, Te, Fe, S, Ti, Zr, Sc, Si, Pt, Nb, Re, Mo, and Hf, a total amount of the at least one alloying element present in the target being at least 100 ppm and less than 10% by weight; the target having a hardness of at least 40 HB.

### Claim 17 (depends on 16)

The target of claim 16 having an average grain size of less than 1 micron.

### Claim 18 (depends on 17)

The target of claim 17 having a grain size uniformity standard deviation throughout the target of less than or equal to about 15% (1-sigma).

### Claim 19 (depends on 17)

The target of claim 17 having a grain size uniformity standard deviation throughout the target of less than or equal to about 10% (1-sigma).

### Claim 20 (depends on 16)

The target of claim 16 having a hardness uniformity standard deviation of less than about 5% (1-sigma) throughout the target.

### Claim 21 (depends on 20)

The target of claim 20 wherein the hardness uniformity standard deviation is less than about 3.5% (1-sigma).

### Claim 22 (depends on 16)

The target of claim 16 wherein the target is monolithic.

### Claim 23 (depends on 16)

The target of claim 16 is diffusion bonded to a backing plate, the diffusion bond having a bond yield strength of greater than about 15 ksi.

### Claim 24 (depends on 16)

The target of claim 16 having an orientation distribution function (ODF) of less than about 15 times random.

### Claim 25 (depends on 16)

The target of claim 16 having an orientation distribution function (ODF) of less than about 5 times random.

### Claim 26 (depends on 16)

The target of claim 16 having a primary grain orientation other than (220).

### Claim 27 (depends on 16)

The target of claim 16 wherein the at least one alloying element is selected from the group consisting of Ag, Al, In, Zn, B, Ga, Mg, Sn, Ge, Ti, and Zr.

### Claim 28 (depends on 16)

The target of claim 16 wherein the total amount of alloying elements is from about 1000 ppm to less than about 2%.

### Claim 29

A copper alloy sputtering target consisting essentially of:
less than or equal to about 99.99% copper, by weight;
at least one alloying element selected from the group consisting of Cd, Ca, Au, Ag, Be, Li, Mg, Al, Pd, Hg, Ni, In, Zn, B, Ga, Mn, Sn, Ge, W, Cr, O, Sb, Ir, P, As, Co, Te, Fe, S, Ti, Zr, Sc, Mo, Si, Re, Pt, Nb, and Hf, a total amount of the at least one alloying element present in the target being at least 100 ppm and less than 10%, by weight; the target having an average grain size of from 1 micron to about 20 micron, and having a grain size uniformity with a standard deviation of less than about 15% (1-sigma) throughout the target.

### Claim 30 (depends on 29)

The target of claim 29 wherein the grain size uniformity standard deviation is less than about 10% (1-sigma).

### Claim 31 (depends on 29)

The target of claim 29 having a hardness of at least about 40 HB.

### Claim 32 (depends on 29)

The target of claim 29 having a hardness uniformity comprising a hardness standard deviation of less than about 5% of 1-sigma throughout the target.

### Claim 33 (depends on 29)

The target of claim 29 wherein the target is monolithic.

### Claim 34 (depends on 29)

The target of claim 29 is diffusion bonded to a backing plate, the diffusion bond having a bond yield strength of greater than about 15 ksi.

### Claim 35 (depends on 29)

The target of claim 29 having an orientation distribution function (ODF) of less than about 15 times random.

### Claim 36 (depends on 29)

The target of claim 29 having an orientation distribution function (ODF) of less than about 5 times random.

### Claim 37 (depends on 29)

The target of claim 29 having a primary grain orientation other than (220).

### Claim 38 (depends on 29)

The target of claim 29 wherein the at least one alloying element is selected from the group consisting of Ag, Al, In, Zn, B, Ga, Mg, Sn, Ge, Ti, and Zr.

### Claim 39 (depends on 29)

The target of claim 29 wherein the total amount of alloying elements is from about 1000 ppm to less than about 2%.

### Claim 40

A monolithic sputtering target consisting essentially of copper and less than or equal to 10% by weight of a total amount of alloying elements.

### Claim 41 (depends on 40)

The monolithic target of claim 40 wherein the total amount of alloying elements comprise at least one element selected from the group consisting of Cd, Ca, Au, Ag, Be, Li, Mg, Al, Pd, Hg, Ni, In, Zn, B, Ga, Mn, Sn, Ge, W, Cr, O, Sb, Ir, P, As, Co, Te, Fe, S, Ti, Zr, Sc, Mo, Si, Re, Pt, Nb, and Hf.

### Claim 42 (depends on 41)

The monolithic target of claim 41 wherein the at least one element is selected from the group consisting of Ag, Al, Sn, and Ti

### Claim 43 (depends on 40)

The monolithic target of claim 40 wherein the total amount of alloying elements is less than or equal to about 2%, by weight.

### Claim 44 (depends on 40)

The monolithic target of claim 40 comprising at least 99.99% copper, by weight.

### Claim 45 (depends on 40)

The monolithic target of claim 40 wherein the target comprises a circular shape having a thickness of about 1 inch.

### Claim 46 (depends on 40)

The monolithic target of claim 40 comprising an average grain size of from about 15 microns to about 50 microns.

### Claim 47

A bonded sputtering target consisting essentially of copper and less than or equal to 10% by weight of a total amount of alloying elements.

### Claim 48 (depends on 47)

The bonded target of claim 47 wherein the total amount of alloying elements comprises at least one element selected from the group consisting of Cd, Ca, Au, Ag, Be, Li, Mg, Al, Pd, Hg, Ni, In, Zn, B, Ga, Mn, Sn, Ge, W, Cr, O, Sb, Ir, P, As, Co, Te, Fe, S, Ti, Zr, Sc, Mo, Si, Re, Pt, Nb, and Hf.

### Claim 49 (depends on 48)

The bonded target of claim 48 wherein the at least one element is selected from the group consisting Ag, Al, Sn, and Ti.

### Claim 50 (depends on 47)

The bonded target of claim 47 wherein the total amount of alloying elements is less than or equal to about 2%, by weight.

### Claim 51 (depends on 47)

The bonded target of claim 47 comprising at least 99.99% copper, by weight.

### Claim 52 (depends on 47)

The bonded target of claim 47 wherein the target comprises a circular shape.

### Claim 53 (depends on 47)

The bonded target of claim 47 comprising an average grain size of less than about 100 microns.

### Claim 54 (depends on 53)

The bonded target of claim 53 wherein the average grain size is from about 15 microns to about 50 microns.

### Claim 55 (depends on 53)

The bonded target of claim 53 wherein the average grain size is less than about 30 microns.

### Claim 56 (depends on 47)

The bonded target of claim 47 wherein the target is diffusion bonded to a backing plate with a bond strength of at least about 15 ksi.

### Claim 57 (depends on 56)

The bonded target of claim 56 wherein the bond strength is at least about 30 ksi

### Claim 58 (depends on 56)

The bonded target of claim 56 wherein the backing plate is a CuCr backing plate.

### Claim 59

A method of forming a monolithic sputtering target, comprising:
providing a copper billet consisting essentially of copper and less than or equal to 10% by weight of a total amount of one or more alloying elements;
heating the billet to a temperature of at least about 900° F. and maintaining the temperature for at least about 45 minutes;
hot-forging the billet with a reduction in height of at least about 50% to form a forged block;
cold rolling the forged block to a reduction of at least about 60% to form a blank;
heating the blank to induce recrystallization and form a final grain distribution having an average grain size less than about 100 microns; and
forming the blank into a monolithic target shape.

### Claim 60 (depends on 59)

The method of claim 59 further comprising water quenching after the hot-forging.

### Claim 61 (depends on 59)

The method of claim 59 wherein the one or more alloying elements comprise one or more elements selected from the group consisting of Cd, Ca, Au, Ag, Be, Li, Mg, Al, Pd, Hg, Ni, In, Zn, B, Ga, Mn, Sn, Ge, W, Cr, O, Sb, Ir, P, As, Co, Te, Fe, S, Ti, Zr, Sc, Mo, Si, Re, Pt, Nb, and Hf.

### Claim 62 (depends on 61)

The method of claim 61 wherein the one or more alloying elements are selected from the group consisting of Ag, Al, Sn, and Ti.

### Claim 63

A method of forming a monolithic sputtering target, comprising:
providing a copper billet comprising at least 99.99% copper, by weight;
heating the billet to a temperature of at least about 900° F. and maintaining the temperature for at least about 45 minutes;
hot-forging the billet with a reduction in height of at least about 50% to form a forged block;
cold rolling the forged block to a reduction of at least about 60% to form a blank;
heating the blank to induce recrystallization and form a final grain distribution having an average grain size less than about 100 microns; and
forming the blank into a monolithic target shape.

### Claim 64 (depends on 63)

The method of claim 63 wherein the average grain size of less than or equal to about 50 microns.

### Claim 65 (depends on 57)

The method of claim 57 wherein the average grain size is less than or equal to about 15 microns.

### Claim 66 (depends on 57)

The method of claim 57 further comprising performing equal channel angular extrusion prior to the cold rolling.

### Claim 67

A method of forming a bonded sputtering target, comprising:
providing a copper billet comprising at least 99.99% copper, by weight;
heating the billet to a temperature of at least about 900° F. and maintaining the temperature for at least about 45 minutes;
hot-forging the billet with a reduction in height of at least about 50% to form a forged block;
cold rolling the forged block to a reduction of at least about 50% to form a blank; and
bonding the blank to a backing plate.

### Claim 68 (depends on 67)

The method of claim 67 wherein the bonding is conducted at a temperature which induces recrystallization and forms a final grain distribution having an average grain size less than about 100 microns.

### Claim 69 (depends on 67)

The method of claim 67 wherein the bonding produces a bond having a strength of at least 15 ksi.

### Claim 70 (depends on 67)

The method of claim 67 wherein the hot-forging comprises:
an initial heating;
a partial height reduction; and
at least one re-heating and additional height reduction.

### Claim 71 (depends on 67)

The method of claim 67, further comprising water quenching after the hot forging.

### Claim 72

A method of forming a bonded sputtering target, comprising:
providing a copper billet consisting essentially of copper and less than or equal to 10% by weight of a total amount of one or more alloying elements;
heating the billet to a temperature of at least about 900° F. and maintaining the temperature for at least about 45 minutes;
hot-forging the billet with a reduction in height of at least about 50% to form a forged block;
cold rolling the forged block to a reduction of at least about 50% to form a blank; and
bonding the blank to a backing plate.

### Claim 73 (depends on 72)

The method of claim 72 wherein the bonding is conducted at a temperature which induces recrystallization and forms a final grain distribution having an average grain size less than about 100 microns

### Claim 74 (depends on 72)

The method of claim 72 wherein the one or more alloying elements comprise one or more elements selected from the group consisting of Cd, Ca, Au, Ag, Be, Li, Mg, Al, Pd, Hg, Ni, In, Zn, B, Ga, Mn, Sn, Ge, W, Cr, O, Sb, Ir, P, As, Co, Te, Fe, S, Ti, Zr, Sc, Mo, Si, Re, Pt, Nb, and Hf.

### Claim 75 (depends on 74)

The method of claim 74 wherein the one or more elements are selected from the group consisting of Ag, Al, Sn, and Ti.

### Claim 76 (depends on 72)

The, method of claim 72, wherein the bonding comprises diffusion bonding to produce a bond having a strength of at least 15 ksi.

### Claim 77 (depends on 72)

The method of claim 72, wherein the hot-forging comprises:
an initial heating;
a partial height reduction; and
at least one re-heating and additional height reduction.

### Claim 78 (depends on 72)

The method of claim 72 further comprising performing equal channel angular extrusion prior to the cold rolling.

### Claim 79

A method of forming a copper-comprising sputtering target, comprising:
providing a Cu billet having a purity of at least 99.99% copper;
hot-forging the Cu billet at a temperature of greater than 300° C. with a reduction in height of at least about 40% to form a forged block;
water quenching the forged block;
performing an extrusion process comprising:
at least four passes of the forged block through equal channel angular extrusion (ECAE); and
a heat-treatment comprising one or both of intermediate annealing between at least some of the at least four passes, and heating ECAE die to a temperature of from about 125° C. to about 225° C. during the extrusion process;
after extrusion process, cold-rolling to a reduction of less than 90% to form a blank; and
forming the blank into a target.

### Claim 80 (depends on 79)

The method of claim 79 further comprising solutionizing the forged block prior to water quenching, the solutionizing comprising heating the forged block to a temperature of at least about 500° C. and maintaining the temperature for at least about 60 minutes.

### Claim 81 (depends on 79)

The method of claim 79 wherein the extrusion process comprises intermediate annealing at a temperature of from about 125° C. to about 225° C. for greater than about 1 hour.

### Claim 82 (depends on 79)

The method of claim 79 further comprising heating the blank to recrystallize the copper and form a final grain distribution within the blank, the final grain distribution having an average grain size of from about 1 to about 20 microns; wherein the forming the blank into a target forms a monolithic target.

### Claim 83 (depends on 79)

The method of claim 79 wherein the forming the blank into a target comprises forming a bonded target.

### Claim 84 (depends on 83)

The method of claim 83 wherein the forming the bonded target comprises bonding the target to a backing plate, the bonding being conducted at a temperature of less than or equal to about 325° C. for a time of less than about 4 hours, the bonding comprising at least one of hipping, roll cladding, soldering and diffusion bonding.

### Claim 85 (depends on 84)

The method of claim 84 wherein the bonding comprises diffusion bonding to form a bond having a bond yield strength of from at least about 10 ksi to about 15 ksi.

### Claim 86 (depends on 79)

The method of claim 79 wherein the average grain size is from 1 micron to about 50 microns.

### Claim 87 (depends on 86)

The method of claim 86 wherein the average grain size is from 5 microns to about 20 microns.

### Claim 88 (depends on 79)

The method of claim 79 wherein a uniform grain size distribution exists throughout an entirety of the blank, the uniform grain size having a standard deviation of less than 15% (1-sigma).

### Claim 89 (depends on 88)

The method of claim 88 wherein the grain size uniformity standard deviation is less than about 10% (1-sigma).

### Claim 90 (depends on 79)

The method of claim 79 wherein the Cu billet has a purity of at least about 99.999% copper.

### Claim 91 (depends on 79)

The method of claim 79 wherein the Cu billet has a purity of at least about 99.9999% copper.

### Claim 92 (depends on 79)

The method of claim 79 wherein the Cu billet has a purity of at least about 99.99995% copper.

### Claim 93 (depends on 79)

The method of claim 79 wherein the at least four passes consists of from four to six passes.

### Claim 94

A method of forming a copper alloy sputtering target, comprising:
providing a Cu billet consisting essentially of less than 99.99% copper and at least one alloying element selected from the group consisting of Cd, Ca, Au, Ag, Be, Li, Mg, Al, Pd, Hg, Ni, In, Zn, B, Ga, Mn, Sn, Ge, W, Cr, O, Sb, Ir, P, As, Co, Te, Fe, S, Ti, Zr, Sc, and Hf, a total amount of the at least one alloying element present in the Cu billet being at least 100 ppm and less than 10% by weight;
hot-forging the Cu billet at a temperature of greater than 300° C. with a reduction in height of at least about 40% to form a forged block;
performing an extrusion process comprising:
at least four passes of the forged block through equal channel angular extrusion (ECAE); and
a heat-treatment comprising one or both of heating ECAE die during the extrusion process, and intermediate annealing at a temperature of from about 120° C. to about 325° C., for a time of at least 1 hour between at least some of the at least four passes;
after the extrusion process, cold-rolling to a reduction of less than about 90% to form a blank; and
forming the blank into a target.

### Claim 95 (depends on 94)

The method of claim 94 wherein the extrusion process comprises heating the ECAE die to a temperature of from about 125° C. to about 325° C.

### Claim 96 (depends on 94)

The method of claim 94 further comprising solutionizing the forged block by heating to a temperature of at least about 500° C. and maintaining the temperature for at least about 60 minutes prior to the extrusion process.

### Claim 97 (depends on 94)

The method of claim 94 wherein the at least four passes consists of from four to six passes.

### Claim 98 (depends on 94)

The method of claim 94 wherein during and after the extruding process the method utilizes only temperatures less than or equal to 350° C., and wherein the forming the, blank into a target comprises forming a monolithic. target.

### Claim 99 (depends on 94)

The method of claim 94 wherein the forming the blank into a target comprises forming a bonded target.

### Claim 100 (depends on 99)

The method of claim 99 further comprising performing a full static recrystallization treatment conducted at a temperature of from about 250° C. to about 500° C. for a time of from about 1 hour to about 8 hours, prior to the forming the bonded target.

### Claim 101 (depends on 99)

The method of claim 99 further comprising performing a full static recrystallization treatment conducted at a temperature of from about 250° C. to about 500° C. for a time of from about 1 hour to about 8 hours after the forming the bonded target.

### Claim 102 (depends on 99)

The method of claim 99 wherein the forming the bonded target comprises bonding the target to a backing plate, the bonding being conducted at a temperature of less than or equal to about 500° C. for a time of less than or equal to about 4 hours, the bonding comprising at least one of hipping, roll cladding, soldering, explosive bonding, frictionless forging and diffusion bonding.

### Claim 103 (depends on 99)

The method of claim 99 wherein the bonding comprises diffusion bonding to form a bond having a bond yield strength of from at least about 10 ksi to about 15 ksi.

### Claim 104 (depends on 94)

The method of claim 94 wherein the average grain size is from 1 micron to about 20 microns.

### Claim 105 (depends on 104)

The method of claim 104 wherein the average grain size is from about 5 microns to about 10 microns.

### Claim 106 (depends on 94)

The method of claim 94 wherein the average grain size is less than 1 micron.

### Claim 107 (depends on 94)

The method of claim 94 wherein a uniform grain size distribution exists throughout an entirety of the blank, the uniform grain size having a standard deviation of less than 15% (1-sigma).

### Claim 108 (depends on 107)

The method of claim 107 wherein the grain size uniformity standard deviation is less than about 10% (1-sigma).

### Claim 109 (depends on 94)

The method of claim 94 further comprising, prior to the extruding process, performing an aging treatment at a temperature of less than about 500° C. to form precipitates having an average precipitate size of less than or equal to about 0.5 micron.