# US 2004/0063569 A1 · Microporous crystalline zeolite material (ITQ-20) and production method thereof

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2004/0063569 A1
- Document ID: US20040063569A1
- Status: Published application
- Kind: A1
- Application number: 10/630,366
- Filed: 2003-07-30
- Published: 2004-04-01
- Earliest claimed: 2001-01-30
- Assignees: Consejo Superior de Investigaciones Cientificas; Universidad Politecnica de Valencia
- Inventors: Avelino Corma Canos; Urbano Diaz Morales; Vicente Fornes Segui
- Web page: https://patentgrep.com/patent/US20040063569A1

## CPC

- C01B 39/04: using at least one organic template directing agent, e.g. an ionic quaternary ammonium compound or an aminated compound
- B01J 29/035: {Microporous crystalline materials not having base exchange properties, such as} silica polymorphs, e.g. silicalites
- B01J 29/04: having base-exchange properties, e.g. crystalline zeolites {(B01J29/005 takes precedence)}
- B01J 29/70: of types characterised by their specific structure not provided for in groups B01J29/08 - B01J29/65
- C01B 33/38: Layered base-exchange silicates, e.g. clays, micas or alkali metal silicates of kenyaite or magadiite type {(activation of naturally occurring clays B01J20/12; pillared layered base-exchange silicates B01J29/049)}
- C01B 37/02: Crystalline silica-polymorphs, e.g. silicalites {dealuminated aluminosilicate zeolites}
- C01B 39/48: using at least one organic template directing agent
- C01B: NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; {METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C}
- B01J: CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS

## Abstract

The invention relates to a microporous crystalline zeolite material having the empirical formula x(M1/nXO2):yYO2:(1−y)SiO2 wherein x has a value less than 0.02; y has a value less than 0.1; M is at least an inorganic cation with a +n charge; X is at least a chemical element having oxidation state +3, preferably selected from the group consisting of Al, Ga, B, Cr, Fe, and Y is at least a chemical element with oxidation state +4, preferably selected from the group consisting of Ge, Ti, Sn, V. The inventive material can be obtained by means of a process comprising: preparing a laminar precursor, crystallized from a reaction mixture; swelling the precursor in a solution in order to obtain a swollen laminar material; which is then washed and dried to obtain a swollen solid; delaminating the solid to obtain a delaminated material in suspension; separating the delaminating material and eliminating the organic remnants by cationic exchange and/or calcination.

## Claims

### Claim 1

A microporous crystalline material of zeolitic nature, characterized in that the material has, in a anhydrous state calcinated at temperatures between 300° C. and 800° C., an X-ray diffraction pattern according to
5 d (Å) (I/IO) *100 32.82 ± 0.02 vs 11.97 ± 0.03 w 10.05 ± 0.04 w 9.39 ± 0.06 m 7.05 ± 0.05 w 6.93 ± 0.02 w 6.56 ± 0.05 w 5.64 ± 0.07 w 4.77 ± 0.08 w 4.27 ± 0.04 W 3.98 ± 0.08 w 3.89 ± 0.08 w 3.72 ± 0.03 w 3.53 ± 0.05 w 3.46 ± 0.07 w 3.34 ± 0.06 w 2.90 ± 0.08 w
wherein
w is a weak relative intensity between 0 and 20%;
m is an average relative intensity between 20 & 40%;
s is an average relative intensity between 40 and 60%;
vs is an average relative intensity between 60 and 100%
and in that it has an empirical formula
x(M1/nXO2):yYO2:(1−y)SiO2
wherein
x has a value less than 0.2;
y has a value less than 0.1:
M is at least one +n charge inorganic cation,
X is at least one chemical element with a +3 oxidation state, preferably selected from the group consisting of Al, Ga, B, Cr and Fe;
Y is at least one chemical element with a +4 oxidation state, preferably selected from the group consisting of Ge, Ti, Sn and V.

### Claim 2 (depends on 1)

A crystalline material according to claim 1, characterized in that
x has a value less than 0.1, preferably less than 0.02,
y has a value less than 0.05, preferably less than 0.02.

### Claim 3 (depends on 2)

A crystalline material according to claim 2, characterized in that x has the value of 0.

### Claim 4 (depends on 1)

A crystalline material according to claim 1, characterized in that M is H.

### Claim 5 (depends on 1)

A crystalline material according to claim 1, characterized in that it has specific surface characteristics measured by N2 adsorption-desorption, with an external surface of at least 100 m2g−1, and preferably with more than 400 m2g−1.

### Claim 6 (depends on 1)

A process to synthesize the crystalline material of claim 1, characterized in that it comprises
a first step wherein a precursor is prepared by subjecting to heating, with or without stirring, at a temperature between 100 and 225° C., preferably between 125 and 200° C., a reaction mixture that contains
a SiO2 source,
optionally a GeO2 source,
optionally a source of at least another tetravalent element Y preferably selected from the group consisting of Ge, Ti, V and Sn, optionally a source of at least another trivalent element X preferably selected from the group consisting of Al, B, Ga, Fe and Cr,
an organic cation 1-methyl-1,4-diazabicyclo[2,2,2]octane,
and water,
wherein the reaction mixture has a composition, in terms of molar ratios of oxides, comprised in the ranges of
ROH/SiO2=0.01-1.0, preferably 0.1-1.0,
M1/nOH/SiO2=0-1.0, preferably 0-0.2,
X2O3/SiO2=0-0.1, preferably 0-05, and more preferably 0-0.01,
YO2/(YO2+SiO2) less than 1, preferably less than 0.1,
H2O/SiO2=0-100, preferably 1-50, wherein
M is at least a +n charge inorganic cation;
X is at least a trivalent element preferably selected from the group consisting of Al, B, Ga. Fe and Cr;
Y is at least a trivalent element preferably selected from the group consisting of Ge, Ti, Sn and V;
R is an organic cation, preferably 1-methyl-1,4-diazabicyclo[2,2,2]octane
until crystallization of the reaction mixture is achieved;
a second stage wherein the precursor is subjected to swelling in a swelling solution in order to obtain a swollen laminar material;
a third stage wherein the swollen laminar material is washed and dried in order to obtain a dry swollen solid;
a fourth stage wherein the dry swollen solid is subjected to at least partial delamination in water in order to obtain a suspension that contains a material at least partially delaminated;
a fifth stage wherein the material at least partially delaminated is separated from the suspension;
a sixth stage wherein the organic wastes are removed from the at least partially delaminated material, by means of a treatment selected from the group consisting of cationic exchange, calcination and combinations thereof.

### Claim 7 (depends on 6)

A process according to claim 6, characterized in that the organic cation 1-methyl-1,4-diazabicyclo[2,2,2]octane is added in the form of a hydroxide and another salt, preferably halide, to the reaction mixture.

### Claim 8 (depends on 1, 6)

A process according to claim 6, characterized in that an amount of crystalline material, preferably with the characteristics of the material of claim 1 as the crystallization promoter is added to the reaction mixture, said amount being comprised between 0.01 to 15%, preferably 0.05 to 5% by weight referred to the total silica added.

### Claim 9

A process according to 6, characterized in that the precursor has an X-ray diffractogram that comprises values corresponding to
6 d (Å) (I/IO) *100 d (Å) (I/IO) *100 11.22 ± 0.02 vs 3.60 ± 0.08 s 10.10 ± 0.03 w 3.52 ± 0.05 vs 8.81 ± 0.05 w 3.42 ± 0.06 s 7.05 ± 0.01 w 3.36 ± 0.04 s 6.30 ± 0.01 m 3.32 ± 0.05 w 5.60 ± 0.02 w 3.30 ± 0.01 w 5.28 ± 0.05 s 3.14 ± 0.07 w 4.98 ± 0.06 s 3.10 ± 0.02 w 4.72 ± 0.01 w 3.09 ± 0.03 w 4.38 ± 0.02 s 3.01 ± 0.01 w 4.21 ± 0.02 s 2.81 ± 0.04 w 3.90 ± 0.03 w 2.61 ± 0.04 w 3.83 ± 0.08 m 3.51 ± 0.05 w 3.73 ± 0.07 m 2.48 ± 0.09 w
wherein
w is a weak relative intensity between 0 and 20%;
m is an average relative intensity between 20 & 40%;
s is an average relative intensity between 40 and 60%;
vs is an average relative intensity between 60 and 100%.

### Claim 10 (depends on 6)

A process according to claim 6, wherein the swelling solution with which the dry swollen solid is obtained, contains organic molecules that are intercalated in order to produce a separation of sheets of the precursor.

### Claim 11 (depends on 10)

A process according to claim 10, characterized in that the organic molecules used in the swelling solution with which the dry swollen solid is obtained are selected between molecules that have a proton acceptor group and a hydrocarbonaceous chain.

### Claim 12 (depends on 10)

A process according to claim 10, characterized in that the organic molecules used in the swelling solution with which the dry swollen solid is obtained are selected from among alkylammonium molecules, with a number of carbon atoms between 4 and 24, preferably between 16 and 19.

### Claim 13 (depends on 10)

A process according to claim 10, characterized in that the organic molecules used in the swelling solution with which the dry swollen solid is obtained are molecules of cetyltrimetylammonium chloride (CTMA+).

### Claim 14 (depends on 6)

A process according to claim 6, characterized in that the swelling solution comprises
a suspension of the precursor in a solid suspension between 10 and up to 50% by weight;
a cetyltrimethylammonium hydroxide solution (OH−, Br−) between 10 up to 50% by weight;
a tetrapropylammonium solution (TPA+) (OH−, Br−) between 20 up to 60% by weight.

### Claim 15 (depends on 6)

A process according to claim 6, characterized in that the swelling solution comprises
a suspension of the solid precursor up to 20% by weight;
a cetyltrimetylammonium hydroxide solution (OH−, Br−) up to 29% by weight;
a tetrapropylammonium solution (OH−, Br−) up to 40% by weight;
with a weight ratio of precursor suspension: cetyltrimethylammonium hydroxide (OH−, Br−) solution: tetrapropylammonium (OH-, Br−) solution of 27:105:33.

### Claim 16 (depends on 13)

A process according to claim 13, characterized in that the dry swollen solid has X-ray diffraction values corresponding to.
7 d (Å) (I/IO) *100 d (Å) (I/IO) *100 37.89 ± 0.02 vs 4.71 ± 0.03 w 14.50 ± 0.02 s 4.23 ± 0.04 m 12.50 ± 0.03 m 4.14 ± 0.08 m 11.73 ± 0.01 w 3.95 ± 0.09 m 10.01 ± 0.04 w 3.86 ± 0.08 m 7.66 ± 0.05 w 3.82 ± 0.09 m 7.36 ± 0.03 w 3.51 ± 0.08 m 6.99 ± 0.06 w 3.43 ± 0.08 w 6.55 ± 0.05 w 3.31 ± 0.05 w 5.98 ± 0.01 w 3.18 ± 0.07 w 5.59 ± 0.08 w 2.88 ± 0.09 w 5.11 ± 0.04 w
wherein
w is a weak relative intensity between 0 and 20%;
m is an average relative intensity between 20 & 40%;
s is an average relative intensity between 40 and 60%;
vs is an average relative intensity between 60 and 100%.

### Claim 17 (depends on 6)

A process according to claim 6, characterized in that the fourth step is carried out at least by means of a technique selected from the group consisting of mechanical stirring, ultrasound, spray-drying, lyophilization and combinations thereof.

### Claim 18 (depends on 6)

A process according to claim 6, characterized in that the suspension that contains the at least partially delaminated material is subjected to flocculation.

### Claim 19 (depends on 6)

A process according to claim 6, characterized in that, in the sixth stage, the at least partially delaminated material is calcinated in an air flow, at a temperature between 300° C. and 800° C. for at least 3 hours.

### Claim 20 (depends on 19)

A process according to claim 19, characterized in that the temperature is between 400° C. and 600° C.