# US 2004/0016318 A1 · Method for making materials having artificially dispersed nano-size phases and articles made therewith

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2004/0016318 A1
- Document ID: US20040016318A1
- Status: Published application
- Kind: A1
- Application number: 10/064,510
- Filed: 2002-07-23
- Published: 2004-01-29
- Earliest claimed: 2002-07-23
- Assignees: General Electric Company
- Inventors: Thomas Martin Angeliu
- Web page: https://patentgrep.com/patent/US20040016318A1

## CPC

- C22C 1/1047: {by mixing and casting liquid metal matrix composites}
- C22C 1/02: by melting {(C22C1/1036 takes precedence)}
- B22F 2999/00: Aspects linked to processes or compositions used in powder metallurgy
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- B22F: WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER (making alloys by powder metallurgy C22C); APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER

## Abstract

A method for forming a nanocomposite material and articles made with the nanocomposite material are presented. The method comprises providing a molten material; providing a nano-sized material, the nano-sized material being substantially inert with respect to the molten material; introducing the nano-sized material into the molten material; dispersing the nano-sized material within the molten material using at least one dispersion technique selected from the group consisting of agitating the molten material using ultrasonic energy to disperse the nano-sized material within the molten material, introducing at least one active element into the molten material to enhance wetting of the nano-sized material by the molten material, and coating the nano-sized material with a wetting agent to promote wetting of the molten metal on the nano-sized material; and solidifying the molten material to form a solid nanocomposite material, the nanocomposite material comprising a dispersion of the nano-sized material within a solid matrix.

## Claims

### Claim 1

A method for forming a nanocomposite material, the method comprising:
providing a molten material;
providing a nano-sized material, said nano-sized material being substantially inert with respect to said molten material;
introducing said nano-sized material into said molten material;
dispersing said nano-sized material within said molten material using at least one dispersion technique selected from the group consisting of agitating said molten material using ultrasonic energy to disperse said nano-sized material within said molten material;
introducing at least one active element into said molten material to enhance wetting of said nano-sized material by said molten material; and
coating said nano-sized material with a wetting agent to promote wetting of said molten metal on said nano-sized material; and
solidifying said molten material to form a solid nanocomposite material, said nanocomposite material comprising a dispersion of said nano-sized material within a solid matrix.

### Claim 2 (depends on 1)

The method of claim 1, wherein introducing said at least one active element comprises introducing a material selected from the group consisting of titanium, zirconium, yttrium, magnesium, hafnium, oxygen, sulfur, and mixtures thereof.

### Claim 3 (depends on 1)

The method of claim 1, wherein introducing said at least one active element comprises introducing at least 0.01 weight percent of said active element into said molten material.

### Claim 4 (depends on 1)

The method of claim 1, wherein providing said molten material comprises providing at least one metal selected from the group consisting of iron, copper, aluminum, nickel, molybdenum, titanium, tin, and mixtures thereof.

### Claim 5 (depends on 1)

The method of claim 1, wherein providing said nano-sized material comprises providing at least one of a ceramic, an intermetallic, and a metal.

### Claim 6 (depends on 5)

The method of claim 5, wherein providing said ceramic comprises providing an oxide.

### Claim 7 (depends on 6)

The method of claim 6, wherein said oxide comprises at least one of aluminum, yttrium, zirconium, and cerium.

### Claim 8 (depends on 5)

The method of claim 5, wherein providing said ceramic comprises providing at least one of a carbide, a nitride, and a boride.

### Claim 9 (depends on 5)

The method of claim 5, wherein providing said intermetallic comprises providing an intermetallic comprising a silicide.

### Claim 10 (depends on 5)

The method of claim 5, wherein providing a metal comprises providing a metal comprising tungsten.

### Claim 11 (depends on 1)

The method of claim 1, wherein providing said nano-sized material comprises providing a nano-sized material wherein at least about 50 percent by volume of said nano-sized material has a length in at least one dimension of less than about 100 nm.

### Claim 12 (depends on 11)

The method of claim 11, wherein said length in said at least one dimension is less than about 30 nm.

### Claim 13 (depends on 1)

The method of claim 1, wherein providing said nano-sized material comprises providing material comprising at least one of spheres, rectangular prisms, cubes, rods, tubes, and plates.

### Claim 14 (depends on 13)

The method of claim 13, wherein at least a portion of said spheres is hollow.

### Claim 15 (depends on 1)

The method of claim 1 , wherein coating said nano-sized material with a wetting agent comprises coating said nano-sized material with a coating material comprising one of titanium, zirconium, yttrium, magnesium, hafnium, and mixtures thereof.

### Claim 16 (depends on 15)

The method of claim 15, wherein said coating material comprises one of a ceramic, an intermetallic, and a metal.

### Claim 17 (depends on 1)

The method of claim 1, wherein coating said nano-sized material comprises coating said nano-sized material with a layer having a thickness of at least a monolayer of said wetting agent.

### Claim 18 (depends on 1)

The method of claim 1, wherein agitating said molten material using ultrasonic energy comprises using ultrasonic energy having a frequency in the range from about 10 kHz to about 40 kHz.

### Claim 19 (depends on 18)

The method of claim 18, wherein said frequency is in the range between about 20 kHz and about 30 kHz.

### Claim 20 (depends on 1)

The method of claim 1, wherein said dispersion of said nano-sized particles comprises an average inter-particle spacing of less than about 100 nm.

### Claim 21 (depends on 20)

The method of claim 20, wherein said average inter-particle spacing is in the range from about 1 nm to about 100 nm.

### Claim 22 (depends on 21)

The method of claim 21, wherein said average interparticle spacing is in the range from about 1 nm to about 50 nm.

### Claim 23 (depends on 1)

The method of claim 1, wherein solidifying said molten material comprises one of
directionally solidifying to form a directionally solidified solid matrix; and
forming a single crystal solid matrix.

### Claim 24 (depends on 1)

The method of claim 1, wherein introducing said nano-sized material comprises introducing said nano-sized material in an amount of up to about 40 volume percent into said molten material.

### Claim 25 (depends on 24)

The method of claim 24, wherein introducing said nano-sized material comprises introducing said nano-sized material in an amount of up to about 5 volume percent into said molten material.

### Claim 26

A method for forming a nanocomposite material, the method comprising:
providing a molten material;
providing a nano-sized material, said nano-sized material being substantially inert with respect to said molten material,
introducing said nano-sized material into said molten material;
dispersing said nano-sized material within said molten material, wherein dispersing comprises the steps of
agitating said molten material using ultrasonic energy to disperse said nano-sized material within said molten material, and
introducing into said molten material at least one active element selected from the group consisting of titanium, zirconium, yttrium, magnesium, hafnium, oxygen, sulfur, and mixtures thereof, to enhance wetting of said nano-sized material by said molten material; and
solidifying said molten material to form a solid nanocomposite material, said nanocomposite material comprising a dispersion of said nano-sized material within a solid matrix, said dispersion comprising an average inter-particle spacing of less than about 100 nm.

### Claim 27

A method for forming a nanocomposite material, the method comprising:
providing a molten material;
providing a nano-sized material, said nano-sized material being substantially inert with respect to said molten material;
introducing said nano-sized material into said molten material;
dispersing said nano-sized material within said molten material, wherein dispersing comprises the steps of
agitating said molten material using ultrasonic energy to disperse said nano-sized material within said molten material,
coating said nano-sized material with a wetting agent comprising one of titanium, zirconium, yttrium, magnesium, hafnium, and mixtures thereof, to promote wetting of said molten metal on said nano-sized material; and
solidifying said molten material to form a solid nanocomposite material, said nanocomposite material comprising a dispersion of said nano-sized material within a solid matrix, said dispersion comprising an average inter-particle spacing of less than about 100 nm.

### Claim 28

A method for forming a nanocomposite material, the method comprising:
providing a molten material;
providing a nano-sized material, said nano-sized material being substantially inert with respect to said molten material;
introducing said nano-sized material into said molten material;
dispersing said nano-sized material within said molten material, wherein dispersing comprises the steps of
agitating said molten material using ultrasonic energy to disperse said nano-sized material within said molten material, and
introducing into said molten material at least one active element selected from the group consisting of titanium, zirconium, yttrium, magnesium, hafnium, oxygen, sulfur, and mixtures thereof, to enhance wetting of said nano-sized material by said molten material, and
coating said nano-sized material with a wetting agent comprising one of titanium, zirconium, yttrium, magnesium, hafnium, and mixtures thereof, to promote wetting of said molten metal on said nano-sized material; and
solidifying said molten material to form a solid nanocomposite material, said nanocomposite material comprising a dispersion of said nano-sized material within a solid matrix, said dispersion comprising an average inter-particle spacing of less than about 100 nm.

### Claim 29

An article manufactured by a method, the method comprising
providing a nanocomposite material, wherein providing said nanocomposite material comprises
providing a molten material;
providing a nano-sized material, said nano-sized material being substantially inert with respect to said molten material;
introducing said nano-sized material into said molten material;
dispersing said nano-sized material within said molten material using at least one dispersion technique selected from the group consisting of
agitating said molten material using ultrasonic energy to disperse said nano-sized material within said molten material,
introducing at least one active element into said molten material to enhance wetting of said nano-sized material by said molten material, and
coating said nano-sized material with a wetting agent to promote wetting of said molten metal on said nano-sized material;
solidifying said molten material to form a solid nanocomposite material, said nanocomposite material comprising a dispersion of said nano-sized material within a solid matrix; and
forming said nanocomposite material into said article.

### Claim 30 (depends on 29)

The article of claim 29, wherein said at least one active element comprises a material selected from the group consisting of titanium, zirconium, yttrium, magnesium, hafnium, oxygen, sulfur, and mixtures thereof.

### Claim 31 (depends on 29)

The article of claim 29, wherein said molten material comprises at least one metal selected from the group consisting of iron, copper, aluminum, nickel, molybdenum, titanium, tin, and mixtures thereof.

### Claim 32 (depends on 29)

The article of claim 29, wherein said nano-sized material comprises at least one of a ceramic, an intermetallic, and a metal.

### Claim 33 (depends on 29)

The article of claim 29, wherein at least about 50 percent by volume of said nano-sized material has a length in at least one dimension of less than about 100 nm.

### Claim 34 (depends on 33)

The article of claim 33, wherein said length in said at least one dimension is less than about 30 nm.

### Claim 35 (depends on 29)

The article of claim 29, wherein said dispersion of said nano-sized particles comprises an average inter-particle spacing of less than about 100 nm.

### Claim 36 (depends on 29)

The article of claim 29, wherein said solid matrix comprises one of a directionally solidified material and a single crystal material.

### Claim 37

An article comprising:
a nanocomposite material, said nano composite material comprising a dispersion of nano-sized material within a solid matrix, said dispersion having a size distribution wherein a size range of said distribution is less than about 20% of a mean particle size of said distribution.

### Claim 38 (depends on 37)

The article of claim 37, wherein said size range is less than about 10% of said mean particle size of said distribution.

### Claim 39 (depends on 37)

The article of claim 37, wherein said matrix comprises at least one active element selected from the group consisting of titanium, zirconium, yttrium, magnesium, hafnium, oxygen, sulfur.

### Claim 40 (depends on 37)

The article of claim 37, wherein said matrix comprises at least one metal selected from the group consisting of iron, copper, aluminum, nickel, molybdenum, titanium, tin, and mixtures thereof.

### Claim 41 (depends on 37)

The article of claim 37, wherein said nano-sized material comprises at least one of a ceramic, an intermetallic, and a metal.

### Claim 42 (depends on 37)

The article of claim 37, wherein said nano-sized material further comprises a coating.

### Claim 43 (depends on 42)

The article of claim 42, wherein said coating comprises one of a ceramic, an intermetallic, and a metal.

### Claim 44 (depends on 37)

The article of claim 37, wherein said dispersion of said nano-sized particles comprises an average inter-particle spacing of less than about 100 nm.

### Claim 45 (depends on 37)

The article of claim 37, wherein said matrix comprises one of a directionally solidified matrix and a single crystal solid matrix.

### Claim 46 (depends on 37)

The article of claim 37, wherein said nano-sized material is present in said nanocomposite material in an amount of up to about 40 volume percent into said molten material.

### Claim 47

An article comprising:
a nanocomposite material, wherein said nanocomposite material comprises
a matrix having a microstructure selected from the group consisting of a directionally solidified microstructure and a single crystal microstructure, and
a dispersion of nano-sized material within said matrix.

### Claim 48 (depends on 47)

The article of claim 47, wherein said matrix comprises at least one active element selected from the group consisting of titanium, zirconium, yttrium, magnesium, hafnium, oxygen, sulfur.

### Claim 49 (depends on 47)

The article of claim 47, wherein said matrix comprises at least one metal selected from the group consisting of iron, copper, aluminum, nickel, molybdenum, titanium, tin, and mixtures thereof.

### Claim 50 (depends on 47)

The article of claim 47, wherein said nano-sized material comprises at least one of a ceramic, an intermetallic, and a metal.

### Claim 51 (depends on 47)

The article of claim 47, wherein said nano-sized material further comprises a coating.

### Claim 52 (depends on 51)

The article of claim 51, wherein said coating comprises one of a ceramic, an intermetallic, and a metal.

### Claim 53 (depends on 47)

The article of claim 47, wherein said dispersion of said nano-sized particles comprises an average inter-particle spacing of less than about 100 nm.

### Claim 54 (depends on 47)

The article of claim 47, wherein said matrix comprises one of a directionally solidified matrix and a single crystal solid matrix.

### Claim 55 (depends on 47)

The article of claim 47, wherein said nano-sized material is present in said nanocomposite material in an amount of up to about 40 volume percent into said molten material.

### Claim 56

An article comprising:
a nanocomposite material, said nanocomposite material comprising a dispersion of nano-sized material within a solidified matrix material, wherein said dispersion of nano-sized material has an average particle size of up to about 100 nm and an interparticle spacing of up to about 100 nm.

### Claim 57 (depends on 56)

The article of claim 56, wherein said matrix comprises at least one active element selected from the group consisting of titanium, zirconium, yttrium, magnesium, hafnium, oxygen, sulfur.

### Claim 58 (depends on 56)

The article of claim 56, wherein said matrix comprises at least one metal selected from the group consisting of iron, copper, aluminum, nickel, molybdenum, titanium, tin, and mixtures thereof.

### Claim 59 (depends on 56)

The article of claim 56, wherein said nano-sized material comprises at least one of a ceramic, an intermetallic, and a metal.

### Claim 60 (depends on 56)

The article of claim 56, wherein said nano sized material further comprises a coating.

### Claim 61 (depends on 60)

The article of claim 60, wherein said coating comprises one of a ceramic, an intermetallic, and a metal.

### Claim 62 (depends on 56)

The article of claim 56, wherein said matrix comprises one of a directionally solidified matrix and a single crystal solid matrix.

### Claim 63 (depends on 56)

The article of claim 56, wherein said nano-sized material is present in said nanocomposite material in an amount of up to about 40 volume percent into said molten material.