# US 2003/0228522 A1 · Method for preparing solid-state polymer zinc-air battery

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2003/0228522 A1
- Document ID: US20030228522A1
- Status: Published application
- Kind: A1
- Application number: 10/219,327
- Filed: 2002-08-16
- Published: 2003-12-11
- Earliest claimed: 2002-06-03
- Assignees: Ming-Chi Institute of Technology
- Inventors: Chun-Chen Yang; Sheng-Jen Lin; Chi-Neng Huang; Jung-Ming Chiu
- Web page: https://patentgrep.com/patent/US20030228522A1

## CPC

- H01M 12/06: with one metallic and one gaseous electrode
- Y02E 60/10: Energy storage using batteries
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

This invention relates to a method for fabricating solid-state alkaline polymer Zn-air battery, which consists of a zinc-gel anode, an air cathode electrode, and alkaline polymer electrolyte. The formulation of said zinc gel anode is similar to that of alkaline Zn—MnO2 battery. The zinc gel anode contains a mixture of electrolytic dendritic zinc powders, KOH electrolyte, gelling agent and small amount of additives. The air cathode electrode is made by carbon gas diffusion electrode, which comprises two layers, namely gas diffusion layer and active layer. The active layer on the electrolyte side uses a high surface area carbon for oxygen reduction reaction and potassium permanganate and MnO2 as catalysts for oxygen reduction. The diffusion layer on the air side has high PTFE content to prevent KOH electrolyte from weeping or climbing. Due to adequate amount of fresh air and oxygen supply, the air cathode electrode can run continuously. Theoretically, the polymer zinc-air battery is an accumulator if the cell has sufficient zinc powder and electrolyte, and the air cathode plays the role of energy transfer.

## Claims

### Claim 1

Process for preparing solid alkaline polymer electrolyte, comprising the steps of:
(a) taking polyvinyl alcohol polymer with molecular weight between 2,000˜120,000 that comprises 10˜20% by weight to mix with water 50˜60% by weight under ambient temperature and in a closed environment;
(b) taking alkaline aqueous solution 15˜25% by weight to mix with water 10˜20% by weight under ambient temperature and in a closed environment;
(c) subsequently mixing the completely dissolved polyvinyl alcohol solution and alkaline metal aqueous together under ambient temperature that viscous solution generated thereof is fully agitated and heating the mixture in a closed container at 50˜100° C. to let it undergo co-polymerization blending, and then letting it cool in atmosphere; and
(d) spreading the cooled viscous polymer on the carrier tray to obtain desired thickness and then placing the tray in temperature/humidity chamber for 30˜60 minutes under the temperature of 40˜80° C. and humidity of 20˜50 RH % to turn it into solid state polymer film, and then leaving the carrier tray in atmosphere where the polymer electrolyte film may be removed with ease.

### Claim 2 (depends on 1)

The process according to claim 1 wherein said alkaline metal solution may be KOH, NaOH, LiOH or its mixture.

### Claim 3 (depends on 1)

The process according to claim 1 wherein said polyvinyl alcohol polymer preferably has average molecular weight of 5,000˜100,000.

### Claim 4 (depends on 1)

The process according to claim 1 wherein glass fiber cloth with thickness of 20 μm ˜400 μm may be added in the process to enhance mechanical strength and thermo-chemical and electrochemical stability of the solid polymer electrolyte.

### Claim 5 (depends on 1)

The process according to claim 1 wherein said polyvinyl alcohol polymer may be added with some micro or nano-particle oxides, such as γ-Al2O3, TiO2, ZrO2 or SiO2.

### Claim 6 (depends on 1)

The process according to claim 1 wherein the optimal condition for temperature/humidity chamber in step (d) is 50° C. temperature and 30 RH %.

### Claim 7

Process for electrolytic dendritic zinc powder with high specific surface area, comprising the steps of:
(a) dissolving 5˜15 wt % zinc oxide powder in alkaline solution under the temperature of 30˜90° C., which is then electrolyzed into dendritic zinc powder under specific conditions with current density of 20˜300 mA/cm2 and with the negative electrode being nickel plate;
(b) scrapping the electroplated zinc powder from the negative electrode, rinsing it with ultra-pure D.I. water, then vibrating it ultrasonically and filtering it; repeating the rinsing 5˜10 times; and
(c) washing the zinc powder thoroughly to prevent the leftover of electroplating fluid that will cause oxidation; drying the zinc powder and storing it in vacuum oven, packing to prevent oxidation.

### Claim 8 (depends on 1)

The process according to claim 1 wherein said alkaline metal solution may be NaOH, KOH, LiOH or its mixture.

### Claim 9

Process for zinc gel anode, comprising the steps of:
(a) weighing proper amount of hydrogen inhibitors, adding in alkaline metal solution and mixing to let the inhibitor distribution uniformly; and
(b) adding 1˜7 wt % dendritic zinc powder into the solution prepared in the foregoing step and vibrating the mixture in ultrasonic device, then adding 0.5˜10 wt % polymer gelling agent and mixing uniformly into gel.

### Claim 10 (depends on 9)

The process according to claim 9 wherein said hydrogen inhibitor may be zinc oxide, indium acetate, magnesium oxide, calcium oxide or barium oxide.

### Claim 11 (depends on 9)

The process according to claim 9 where said polymer gelling agent may be CMC, PVA, starch, poly-acrylic polymer gelling agent or cellulose, etc.

### Claim 12 (depends on 9)

The process according to claim 9 wherein the optimum amount of said gelling agent is 1˜2 wt %.

### Claim 13

Process for diffusion layer of air cathode electrode, comprising the steps of:
(a) weighing proper amount of dispersing agent Triton-X, polytetraflouroethylene (PTFE) and water and mixing them uniformly, and then putting the mixture together with the vessel into ultrasonic device to mix the mixture uniformly;
(b) weighing hydrophobic acetylene carbon powder and adding it into the aforesaid mixture, mixing with ultrasonic device, and then drying the resulting material in vacuum oven to remove the H2O completely;
(c) grinding the material after drying and weighing the needed quantity according to the size of air cathode electrode; and
(d) placing a nickel screen collector in the die and coating the aforesaid material uniformly on said nickel screen, placing the die in thermal press to sinter the material, then putting the hot die in the cooler and removing the diffusion layer after cooling.

### Claim 14

process for air cathode electrode, comprising the steps of:
(1) weighing hydrophilic carbon powder XC-72R and adding in proper amount of catalysts of KMnO4 and MnO2;
(2) weighing PTFE-30 and water and using ultrasonic oscillator to mix PTFE and water uniformly;
(3) mixing the resulting solutions in steps (a) and (b) above and vibrating ultrasonically, then adding in proper amount of alcohol solvent, agitating and vibrating with the aid of ultrasonic device; and
(4) spraying needed amount of resulting solution above on the diffusion layer, subjecting air cathode electrode with active layer sprayed on to high-temperature sintering at 320-350° C., then letting it cool under constant pressure to complete the making of air electrode.