# US 2003/0216006 A1 · Method of improving HDP fill process

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2003/0216006 A1
- Document ID: US20030216006A1
- Status: Published application
- Kind: A1
- Application number: 10/150,843
- Filed: 2002-05-17
- Published: 2003-11-20
- Earliest claimed: 2002-05-17
- Assignees: Micron Technology, Inc.
- Inventors: Li Li; Weimin Li; Gurtej S. Sandhu
- Web page: https://patentgrep.com/patent/US20030216006A1

## CPC

- C23C 16/4408: {by purging residual gases from the reaction chamber or gas lines}
- C23C 16/045: {Coating cavities or hollow spaces, e.g. interior of tubes; Infiltration of porous substrates}
- C23C 16/402: {Silicon dioxide}
- H10W 10/014: {using trench refilling with dielectric materials, e.g. shallow trench isolations}
- H10W 10/17: formed using trench refilling with dielectric materials, e.g. shallow trench isolations
- H10P 14/6336: {in the presence of a plasma [PECVD]}
- H10P 14/6339: {deposition by cyclic CVD, e.g. ALD, ALE or pulsed CVD}
- H10P 14/6682: {the compound being a silane, e.g. disilane, methylsilane or chlorosilane}
- H10P 14/69215: {the material being a silicon oxide, e.g. SiO2}
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- H10W: GENERIC PACKAGES, INTERCONNECTIONS, CONNECTORS OR OTHER CONSTRUCTIONAL DETAILS OF DEVICES COVERED BY CLASS H10
- H10P: GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10

## Abstract

A method for depositing a dielectric in a trench on a semiconductor substrate is provided. The dielectric is deposited by using an HDP-CVD system and performing a deposition of first and second layers of dielectric material. A first inert gas is utilized during the deposition of the first layer, and a second inert gas is utilized during the deposition of the second layer. Generally, a purge step is performed between the deposition of the first and second layers. The resulting dielectric layers are substantially free of voids and have low particle counts. Structures utilizing the filled trenches are also disclosed.

## Claims

### Claim 1

A method for filling a trench in a layer disposed in a process chamber comprising:
providing a semiconductor layer having at least one trench therein;
flowing a first precursor gas and a first inert gas into said process chamber and forming a first plasma therein, wherein said first inert gas is selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
depositing a first layer of trench-filling material from said first plasma into said at least one trench;
flowing a second precursor gas and second inert gas into said process chamber and forming a second plasma therein, wherein said second inert gas is selected from the group consisting of helium, neon, argon, and krypton and combinations thereof; and
depositing a second layer of trench-filling material from said second plasma to substantially fill said at least one trench.

### Claim 2 (depends on 1)

The method as claimed in claim 1 wherein said first and second inert gases are selected to be different inert gases.

### Claim 3 (depends on 1)

The method as claimed in claim 1 wherein said first inert gas is selected from the group consisting of helium and neon and combinations thereof, and wherein said second inert gas is selected from the group consisting of argon and krypton and combinations thereof.

### Claim 4 (depends on 1)

The method as claimed in claim 1 wherein said layer comprises a semiconductor substrate.

### Claim 5 (depends on 1)

The method as claimed in claim 1 wherein said layer comprises silicon.

### Claim 6 (depends on 1)

The method as claimed in claim 1 wherein said first and second precursor gas comprises a silicon precursor gas and an oxygen precursor gas and wherein said trench filling material comprises silicon dioxide.

### Claim 7 (depends on 1)

The method as claimed in claim 1 further comprising purging said process chamber of said first inert gas after said deposition of said first layer.

### Claim 8 (depends on 7)

The method as claimed in claim 7 wherein said step of purging comprises terminating said first plasma after said deposition of said first layer.

### Claim 9 (depends on 7)

The method as claimed in claim 7 wherein said step of purging comprises forming an oxygen plasma in said deposition chamber after said deposition of said first layer.

### Claim 10 (depends on 7)

The method as claimed in claim 7 wherein said step of purging comprises venting said first inert gas out of said process chamber after said deposition of said first layer.

### Claim 11

A method for a filling a trench in a layer comprising:
providing a semiconductor layer having at least one trench therein;
placing said semiconductor layer in a first process chamber;
flowing a first precursor gas and a first inert gas into said first process chamber and forming a first plasma therein, wherein said first inert gas is selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
depositing a first layer of trench-filling material from said first plasma into said at least one trench;
placing said semiconductor layer in a second process chamber;
flowing a second precursor gas and a second inert gas into said second process and forming a second plasma therein, wherein said second inert gas is selected from the group consisting of helium, neon, argon, and krypton and combinations thereof; and
depositing a second layer of trench-filling material from said second plasma so as to substantially fill said at least one gap.

### Claim 12 (depends on 11)

The method as claimed in claim 11 wherein said first inert gas is selected from the group consisting of helium and neon and combinations thereof, and wherein said second inert gas is selected from the group consisting of argon and krypton and combinations thereof.

### Claim 13 (depends on 11)

The method as claimed in claim 11 wherein said first and second precursor gas comprises a silicon precursor gas and an oxygen precursor gas and wherein said trench-filling material comprises silicon dioxide.

### Claim 14

A method for filling a trench in a substrate disposed in a process chamber comprising:
providing a semiconductor substrate having at least one trench therein;
flowing a first precursor gas comprising a silicon precursor gas and an oxygen precursor gas and a first inert gas into said process chamber and forming a first plasma therein, wherein said first inert gas is selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
depositing a first layer of silicon dioxide from said first plasma into said at least one trench;
purging said process chamber of said first inert gas by terminating said first plasma after said deposition of said first layer;
flowing a second precursor gas comprising a silicon precursor gas and an oxygen precursor gas and a second inert gas into said process chamber and forming a second plasma therein, wherein said second inert gas is selected from the group consisting of helium, neon, argon, and krypton and combinations thereof; and
depositing a second layer of silicon dioxide from said second plasma to substantially fill said at least one trench.

### Claim 15 (depends on 14)

The method as claimed in claim 14 wherein said first inert gas is selected from the group consisting of helium and neon and combinations thereof, and wherein said second inert gas is selected from the group consisting of argon and krypton and combinations thereof.

### Claim 16

A method for filling a trench in a substrate disposed in a process chamber comprising:
providing a semiconductor substrate having at least one trench therein;
flowing a first precursor gas comprising a silicon precursor gas and an oxygen precursor gas and a first inert gas into said process chamber and forming a first plasma therein, wherein said first inert gas is selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
depositing a first layer of silicon dioxide from said first plasma into said at least one trench;
purging said process chamber of said first inert gas by forming an oxygen plasma in said process chamber after said deposition of said first layer;
flowing a second precursor gas comprising a silicon precursor gas and an oxygen precursor gas and a second inert gas into said process chamber and forming a second plasma therein, wherein said second inert gas is selected from the group consisting of helium, neon, argon, and krypton and combinations thereof; and
depositing a second layer of silicon dioxide from said second plasma to substantially fill said at least one trench.

### Claim 17 (depends on 16)

The method as claimed in claim 16 wherein said first inert gas is selected from the group consisting of helium and neon and combinations thereof, and wherein said second inert gas is selected from the group consisting of argon and krypton and combinations thereof.

### Claim 18

A method for filling a trench in a substrate disposed in a process chamber comprising:
providing a semiconductor substrate having at least one trench therein;
flowing a first precursor gas comprising a silicon precursor gas and an oxygen precursor gas and a first inert gas into said process chamber and forming a first plasma therein, wherein said first inert gas is selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
depositing a first layer of silicon dioxide from said first plasma into said at least one trench;
purging said process chamber of said first inert gas by venting said first inert gas out of said process chamber;
flowing a second precursor gas comprising a silicon precursor gas and an oxygen precursor gas and a second inert into said process chamber and forming a second plasma therein, wherein said second inert gas is selected from the group consisting of helium, neon, argon, and krypton and combinations thereof; and
depositing a second layer of silicon dioxide from said second plasma to substantially fill said at least one trench.

### Claim 19 (depends on 18)

The method as claimed in claim 18 wherein said first inert gas is selected from the group consisting of helium and neon and combinations thereof, and wherein said second inert gas is selected from the group consisting of argon and krypton and combinations thereof.

### Claim 20

A method for filling a trench in a substrate comprising:
providing a semiconductor substrate having at least one trench therein;
placing said semiconductor substrate in a first process chamber;
flowing a first precursor gas comprising a silicon precursor gas and an oxygen precursor gas and a first inert gas into said first process chamber and forming a first plasma therein, wherein said first inert gas is selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
depositing a first layer of silicon dioxide from said first plasma into said at least one trench;
placing said semiconductor substrate in a second process chamber;
flowing a second precursor gas comprising a silicon precursor gas and an oxygen precursor gas and a second inert gas into said second process chamber and forming a second plasma therein, wherein said second inert gas comprises helium, neon, argon, and krypton and combinations thereof; and
depositing a second layer of silicon dioxide from said second plasma to substantially fill said at least one trench.

### Claim 21 (depends on 20)

The method as claimed in claim 20 wherein said first inert gas is selected from the group consisting of helium and neon and combinations thereof, and wherein said second inert gas is selected from the group consisting of argon and krypton and combinations thereof.

### Claim 22

A method for filling a trench in a substrate disposed in a process chamber comprising:
providing a semiconductor substrate having at least one trench therein;
flowing a first precursor gas comprising silane and molecular oxygen and a first inert gas selected from the group consisting of helium and neon and combinations thereof into said process chamber, wherein said silane is flowed into said process chamber at a flow rate of about 1-150 sccm, said molecular oxygen is flowed into said process chamber at a flow rate of about 10-300 sccm and said first inert gas is flowed into said chamber at a flow rate of about 1-2000 sccm;
forming a first plasma in said process chamber;
depositing a first layer of silicon dioxide from said first plasma into said at least one trench;
purging said first inert gas from said process chamber by terminating said first plasma after said deposition of said first layer;
flowing a second precursor gas comprising silane and molecular oxygen and a second inert gas selected from the group consisting of argon and krypton and combinations thereof into said process chamber, wherein said silane is flowed into said process chamber at a flow rate of about 1-150 sccm, said oxygen is flowed into said process chamber at a flow rate of about 10-300 sccm and said second inert gas is flowed into said chamber at a flow rate of about 1-2000 sccm;
forming a second plasma in said process chamber; and
depositing a second layer of silicon dioxide from said second plasma to substantially fill said at least one trench.

### Claim 23 (depends on 22)

The method as claimed in claim 22 wherein said first inert gas is flowed into said chamber at a rate of about 200 sccm and said second inert gas is flowed into said chamber at a rate of about 200 sccm.

### Claim 24

A method for filling a trench in a substrate disposed in a process chamber comprising:
providing a semiconductor substrate having at least one trench therein;
flowing a first precursor gas comprising silane and molecular oxygen and a first inert gas selected from the group consisting of helium and neon and combinations thereof into said process chamber, wherein said silane is flowed into said process chamber at a flow rate of about 1-150 sccm, said molecular oxygen is flowed into said process chamber at a flow rate of about 10-300 sccm and said first inert gas is flowed into said chamber at a flow rate of about 1-2000 sccm;
forming a first plasma in said process chamber;
depositing a first layer of SiO2 from said first plasma into said at least one trench;
purging said first inert gas from said process chamber by forming an oxygen plasma in said process chamber after said deposition of said first layer;
flowing a second precursor gas comprising silane and molecular oxygen and a second inert gas selected from the group consisting of argon and krypton and combinations thereof into said process chamber, wherein said silane is flowed into said process chamber at a flow rate of about 1-150 sccm, said molecular oxygen is flowed into said process chamber at a flow rate of about 10-300 seem and said second inert gas is flowed into said chamber at a flow rate of about 1-2000 sccm;
forming a second plasma in said process chamber; and
depositing a second layer of silicon dioxide from said second plasma to substantially fill said at least one trench.

### Claim 25 (depends on 24)

The method as claimed in claim 24 wherein said first inert gas is flowed into said chamber at a rate of about 200 sccm and said second inert gas is flowed into said chamber at a rate of about 200 sccm.

### Claim 26

A method for filling a trench a substrate disposed in a process chamber comprising:
providing a semiconductor substrate having at least one trench therein;
flowing a first precursor gas comprising silane and oxygen and a first inert gas selected from the group consisting of helium and neon and combinations thereof into said process chamber, wherein said silane is flowed into said process chamber at a flow rate of about 1-150 seem, said oxygen is flowed into said process chamber at a flow rate of about 10-300 sccm and said first inert gas is flowed into said chamber at a flow rate of about 1-2000 sccm;
forming a first plasma in said process chamber;
depositing a first layer of silicon dioxide from said first plasma into said at least one trench;
purging said first inert gas from said process chamber by venting said first inert gas from said process chamber after said deposition of said first layer;
flowing a second precursor gas comprising silane and molecular oxygen and a second inert gas selected from the group consisting of argon and krypton and combinations thereof into said process chamber, wherein said silane is flowed into said process chamber at a flow rate of about 1-150 sccm, said molecular oxygen is flowed into said process chamber at a flow rate of about 10-300 sccm and said second inert gas is flowed into said chamber at a flow rate of about 1-2000 sccm;
forming a second plasma in said process chamber; and
depositing a second layer of silicon dioxide from said second plasma to substantially fill said at least one trench.

### Claim 27 (depends on 26)

The method as claimed in claim 26 wherein said first inert gas is flowed into said chamber at a rate of about 200 sccm and said second inert gas is flowed into said chamber at a rate of about 200 sccm.

### Claim 28

A method for filling a trench in a substrate comprising:
providing a semiconductor substrate having at least one trench therein;
placing said semiconductor substrate in a first process chamber;
flowing a first precursor gas comprising silane and molecular oxygen and a first inert gas selected from the group consisting of helium and neon and combinations thereof into said first process chamber, wherein said silane is flowed into said process chamber at a flow rate of about 1-150 sccm, said molecular oxygen is flowed into said process chamber at a flow rate of about 10-300 sccm and said first inert gas is flowed into said chamber at a flow rate of about 1-2000 seem;
forming a first plasma in said first process chamber;
depositing a first layer of silicon dioxide from said first plasma into said at least one trench;
placing said semiconductor substrate in a second process chamber;
flowing a second precursor gas comprising silane and molecular oxygen and a second inert gas consisting of argon and krypton and combinations thereof into said second process chamber, wherein said silane is flowed into said process chamber at a flow rate of about 1-150 sccm, said molecular oxygen is flowed into said process chamber at a flow rate of about 10-300 sccm and said second inert gas is flowed into said chamber at a flow rate of about 1-2000 sccm;
forming a second plasma in said second process chamber; and
depositing a second layer of silicon dioxide from said second plasma to substantially fill said at least one trench.

### Claim 29 (depends on 28)

The method as claimed in claim 28 wherein said first inert gas is flowed into said first chamber at a rate of about 200 sccm and said second inert gas is flowed into said second chamber at a rate of about 200 sccm.

### Claim 30

A method of forming a silicon dioxide layer filling trenches in a semiconductor wafer by HDP-CVD comprising:
forming a first plasma, wherein said first plasma contains at least a silicon precursor gas, an oxygen precursor gas and a first inert gas selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
exposing said wafer to said first plasma, wherein said step of exposing said wafer to said first plasma causes deposition of a first layer of silicon dioxide in said trenches in said wafer;
forming a second plasma, wherein said second plasma contains at least a silicon precursor gas, an oxygen precursor gas and a second inert gas selected from the group consisting of helium, neon, argon, and krypton and combinations thereof, wherein said second inert gas is selected to be different from said first inert gas; and
exposing said wafer to said second plasma, wherein said step of exposing said wafer to said second plasma causes deposition of a second layer of silicon dioxide substantially filling said trenches in said wafer.

### Claim 31

A method of forming a silicon dioxide layer filling trenches in a semiconductor wafer by HDP-CVD comprising:
forming a first plasma, wherein said first plasma contains at least a silicon precursor gas, an oxygen precursor gas and a first inert gas selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
exposing said wafer to said first plasma, wherein said step of exposing said wafer to said first plasma causes deposition of a first layer of silicon dioxide in said trenches in said wafer;
terminating said first plasma;
forming a second plasma after said termination of said first plasma, wherein said second plasma contains at least a silicon precursor gas, an oxygen precursor gas and a second inert gas selected from the group consisting of helium, neon, argon, and krypton and combinations thereof, wherein said second inert gas is selected to be different from said first inert gas; and
exposing said wafer to said second plasma, wherein said step of exposing said wafer to said second plasma causes deposition of a second layer of silicon dioxide substantially filling said trenches in said wafer.

### Claim 32

A method of forming a silicon dioxide layer filling trenches in a semiconductor wafer by HDP-CVD comprising:
forming a first plasma, wherein said first plasma contains at least a silicon precursor gas, an oxygen precursor gas and a first inert gas selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
exposing said wafer to said first plasma, wherein said step of exposing said wafer to said first plasma causes deposition of a first layer of silicon dioxide in said trenches in said wafer;
forming an oxygen plasma;
terminating said oxygen plasma;
forming a second plasma after said termination of said oxygen plasma, wherein said second plasma contains at least a silicon precursor gas, an oxygen precursor gas and a second inert gas selected from the group consisting of helium, neon, argon, and krypton and combinations thereof, wherein said second inert gas is selected to be different from said first inert gas; and
exposing said wafer to said second plasma, wherein said step of exposing said wafer to said second plasma causes deposition of a second layer of silicon dioxide substantially filling said trenches in said wafer.

### Claim 33

A method of filling trenches in a substrate comprising:
creating a first plasma in a process chamber, wherein said first plasma comprises a silicon precursor gas, an oxygen precursor gas and a first inert gas selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
depositing a first layer of trench-filling material into said trenches in said substrate;
purging said process chamber of said first inert gas;
creating a second plasma in said process chamber, wherein said second plasma comprises a silicon precursor gas, an oxygen precursor gas and a second inert gas selected from the group consisting of helium, neon, argon, and krypton and combinations thereof; and
depositing a second layer of trench-filling material substantially filling said trenches in said substrate.

### Claim 34 (depends on 33)

The method as claimed in claim 33 wherein said first inert gas is selected from the group consisting of helium and neon and combinations thereof, and wherein said second inert gas is selected from the group consisting of argon and krypton.

### Claim 35 (depends on 33)

The method as claimed in claim 33 wherein said step of purging comprises venting said process chamber.

### Claim 36 (depends on 33)

The method as claimed in claim 33 wherein said step of purging comprises creating an oxygen plasma in said process chamber after said deposition of said first layer.

### Claim 37 (depends on 33)

The method as claimed in claim 33 wherein said step of purging comprises terminating said first plasma after said deposition of said first layer.

### Claim 38

A method of filling trenches in a substrate comprising:
placing said substrate in a first process chamber;
creating a first plasma in said first process chamber, wherein said first plasma comprises a silicon precursor gas, an oxygen precursor gas and a first inert gas selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
depositing a first layer of trench-filling material into said trenches in said substrate;
placing said substrate in a second process chamber;
creating a second plasma in said second process chamber, wherein said second plasma comprises a silicon precursor gas, an oxygen precursor gas and a second inert gas selected from the group consisting of helium, neon, argon, and krypton and combinations thereof; and
depositing a second layer of trench-filling material substantially filling said trenches in said substrate.

### Claim 39 (depends on 38)

The method as claimed in claim 38 wherein said first inert gas is selected from the group consisting of helium and neon and combinations thereof, and wherein said second inert gas is selected from the group consisting of argon and krypton.

### Claim 40

A method of filling shallow trench isolation trenches with silicon dioxide comprising:
providing a semiconductor substrate having shallow trench isolation trenches;
placing said semiconductor substrate in a process chamber;
creating a first plasma comprising a silicon precursor gas, an oxygen precursor gas and a first inert gas selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
depositing a first silicon dioxide layer in said shallow trench isolation trenches;
purging said process chamber of said first inert gas; and
creating a second plasma comprising a silicon precursor gas, an oxygen precursor gas and a second inert gas selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
depositing a second silicon dioxide layer substantially filling said shallow trench isolation trenches, wherein said first and second silicon dioxide layers are substantially free of voids.

### Claim 41 (depends on 40)

The method as claimed in claim 40 wherein said first inert gas is selected from the group consisting of helium and neon and combinations thereof, and wherein said second inert gas is selected from the group consisting of argon and krypton.

### Claim 42 (depends on 40)

The method as claimed in claim 40 wherein said step of purging comprises terminating said first plasma after said deposition of said first layer.

### Claim 43 (depends on 40)

The method as claimed in claim 40 wherein said step of purging comprises forming an oxygen plasma in said deposition chamber after said deposition of said first layer.

### Claim 44 (depends on 40)

The method as claimed in claim 40 wherein said step of purging comprises venting said first inert gas out of said process chamber after said deposition of said first layer.

### Claim 45

A trench isolation structure formed in a semiconductor device comprising:
a semiconductor substrate;
a plurality of trenches formed in said semiconductor substrate, each said trench:
being defined by a pair of sidewalls and a bottom wall; and
being filled with a silicon dioxide layer substantially free of voids, wherein said silicon dioxide layer is deposited by:
placing said semiconductor substrate in a process chamber;
creating a first plasma in said process chamber, wherein said first plasma comprises a silicon precursor gas, an oxygen precursor gas and a first inert gas selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
depositing a first layer of silicon dioxide into said trench;
purging said process chamber of said first inert gas;
creating a second plasma in said process chamber, wherein said second plasma comprises a silicon precursor gas, an oxygen precursor gas and second inert gas selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
depositing a second layer of silicon dioxide substantially filling said trench.

### Claim 46 (depends on 45)

The method as claimed in claim 45 wherein said first inert gas is selected from the group consisting of helium and neon and combinations thereof, and wherein said second inert gas is selected from the group consisting of argon and krypton.

### Claim 47

A trench isolation structure formed in a semiconductor device comprising:
a semiconductor substrate;
a plurality of trenches formed in said semiconductor substrate, each said trench:
being defined by a pair of sidewalls and a bottom wall; and
being filled with a silicon dioxide layer substantially free of voids.

### Claim 48

A trench isolation structure formed in a semiconductor device comprising:
a semiconductor substrate;
a plurality of trenches formed in said semiconductor substrate, each said trench
being defined by a pair of sidewalls and a bottom wall;
being filled with a first silicon dioxide layer substantially free of voids that is deposited conformally on said sidewalls and said bottom wall by:
placing said semiconductor substrate in a process chamber;
creating a first plasma in said process chamber, wherein said first plasma comprises a silicon precursor gas, an oxygen precursor gas and a first inert gas selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
depositing said first layer of silicon dioxide into said trench; and
purging said process chamber;
being filled with a second silicon dioxide layer substantially free of voids that is deposited to substantially fill said trench by:
creating a second plasma in said process chamber, wherein said second plasma comprises a silicon precursor gas, an oxygen precursor gas and a second inert gas selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
depositing said second layer of silicon dioxide.

### Claim 49 (depends on 48)

The method as claimed in claim 48 wherein said first inert gas is selected from the group consisting of helium and neon and combinations thereof, and wherein said second inert gas is selected from the group consisting of argon and krypton.

### Claim 50

A trench isolation structure formed in a semiconductor device comprising:
a semiconductor substrate;
a plurality of trenches formed in said semiconductor substrate, each said trench:
being defined by a pair of sidewalls and a bottom wall; and
being filled with a silicon dioxide layer substantially free of voids, wherein said silicon dioxide layer is deposited by:
placing said semiconductor substrate in a process chamber;
creating a first plasma in said process chamber, wherein said first plasma comprises a silicon precursor gas, an oxygen precursor gas and a first inert gas selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
depositing a first layer of silicon dioxide into said trench;
purging said process chamber of said first inert gas by terminating said first plasma;
creating a second plasma in said process chamber, wherein said second plasma comprises a silicon precursor gas, an oxygen precursor gas and a second inert gas selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
depositing a second layer of silicon dioxide substantially filling said trench.

### Claim 51 (depends on 50)

The method as claimed in claim 50 wherein said first inert gas is selected from the group consisting of helium and neon and combinations thereof, and wherein said second inert gas is selected from the group consisting of argon and krypton.

### Claim 52

A trench isolation structure formed in a semiconductor device comprising:
a semiconductor substrate;
a plurality of trenches formed in said semiconductor substrate, each said trench:
being defined by a pair of sidewalls and a bottom wall; and
being filled with a silicon dioxide layer substantially free of voids, wherein said silicon dioxide layer is deposited by:
placing said semiconductor substrate in a process chamber;
creating a first plasma in said process chamber, wherein said first plasma comprises a silicon precursor gas, an oxygen precursor gas and a first inert gas comprising helium, neon, argon, and krypton and combinations thereof;
depositing a first layer of silicon dioxide into said trench;
purging said process chamber of said first inert gas by forming an oxygen plasma in said process chamber;
creating a second plasma in said process chamber, wherein said second plasma comprises a silicon precursor gas, an oxygen precursor gas and second inert gas comprising helium, neon, argon, and krypton and combinations thereof;
depositing a second layer of silicon dioxide substantially filling said trench.

### Claim 53 (depends on 52)

The method as claimed in claim 52 wherein said first inert gas is selected from the group consisting of helium and neon and combinations thereof, and wherein said second inert gas is selected from the group consisting of argon and krypton.

### Claim 54

A trench isolation structure formed in a semiconductor device comprising:
a semiconductor substrate;
a plurality of trenches formed in said semiconductor substrate, each said trench:
being defined by a pair of sidewalls and a bottom wall; and
being filled with a silicon dioxide layer substantially free of voids, wherein said silicon dioxide layer is deposited by:
placing said semiconductor substrate in a process chamber;
creating a first plasma in said process chamber, wherein said first plasma comprises a silicon precursor gas, an oxygen precursor gas and a first inert gas selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
depositing a first layer of silicon dioxide into said trench;
purging said process chamber of said first inert gas by venting said process chamber;
creating a second plasma in said process chamber, wherein said second plasma comprises a silicon precursor gas, an oxygen precursor gas and second inert gas selected from the group consisting of helium, neon, argon, and krypton and combinations thereof;
depositing a second layer of silicon dioxide substantially filling said trench.

### Claim 55 (depends on 54)

The method as claimed in claim 54 wherein said first inert gas is selected from the group consisting of helium and neon and combinations thereof, and wherein said second inert gas is selected from the group consisting of argon and krypton.