# US 2003/0070936 A1 · Light metal anodization

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2003/0070936 A1
- Document ID: US20030070936A1
- Status: Published application
- Kind: A1
- Application number: 10/162,965
- Filed: 2002-06-05
- Published: 2003-04-17
- Earliest claimed: 2001-10-02
- Assignees: Henkel Kommanditgesellschaft auf Aktien
- Inventors: Shawn E. Dolan
- Web page: https://patentgrep.com/patent/US20030070936A1

## CPC

- C25D 11/30: of magnesium or alloys based thereon
- C25D 11/06: characterised by the electrolytes used
- C25D: PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR

## Abstract

Using pulsed current and relatively low average voltages, articles containing light metals such as magnesium may be rapidly anodized to form protective surface coatings. The anodizing solutions employed may contain phosphate, permanganate, silicate, zirconate, vanadate, titanate, hydroxide, alkali metal fluoride and/or complex fluoride, optionally with other components present.

## Claims

### Claim 1

A method of forming a protective coating on a surface of a light metal-containing article, said method comprising:
A) providing an anodizing solution comprised of water and one or more additional components selected from the group consisting of:
a) water-soluble and water-dispersible oxysalts containing at least one element selected from the group consisting of P, Si, Mn, Zr, Ti, V and Hf, or
b) water-soluble and water-dispersible complex fluorides of elements selected from the group consisting of Ti, Zr, Hf, Si, Sn, Al, Ge and B;
c) water-soluble and water-dispersible alkali metal fluorides; and
d) water-soluble and water-dispersible alkali metal hydroxides;
B) providing a cathode in contact with said anodizing solution;
C) placing said light metal-containing article as an anode in said anodizing solution; and
D) passing a pulsed current having an average voltage of not more than 250 volts between the anode and cathode though said anodizing solution for a time effective to form said protective coating on said surface.

### Claim 2 (depends on 1)

The method of claim 1 wherein the light metal-containing article is comprised of magnesium.

### Claim 3 (depends on 1)

The method of claim 1 wherein the light metal-containing article is comprised of aluminum.

### Claim 4 (depends on 1)

The method of claim 1 wherein said anodizing solution is maintained at a temperature of from 5° C. to 90° C. during step (D).

### Claim 5 (depends on 1)

The method of claim 1 wherein said pulsed current has an average voltage of not more than 200 volts.

### Claim 6 (depends on 1)

The method of claim 1 wherein a visible light-emitting discharge is generated during step (D).

### Claim 7 (depends on 1)

The method of claim 1 wherein during step (D) said protective coating is formed at a rate of at least 1 micron thickness per minute.

### Claim 8 (depends on 1)

The method of claim 1 wherein during step (D) said protective coating is formed at a rate of at least 5 microns thickness per minute.

### Claim 9 (depends on 1)

The method of claim 1 wherein said pulsed current has an average voltage of not more than 175 volts.

### Claim 10 (depends on 1)

The method of claim 1 wherein said pulsed current is direct current.

### Claim 11 (depends on 1)

The method of claim 1 wherein the anodizing solution is essentially free of ammonia, chromium, permanganate, borate, sulfate, free fluoride and free chloride.

### Claim 12 (depends on 1)

The method of claim 1 wherein the anodizing solution is comprised of water and a concentration of phosphorus atoms in the form of phosphate that is at least 0.3 M.

### Claim 13 (depends on 1)

The method of claim 1 wherein the anodizing solution is comprised of water and phosphate, but is essentially free of ammonia and amines.

### Claim 14 (depends on 1)

The method of claim 1 wherein the anodizing solution is comprised of water, a concentration of phosphorus atoms in the form of phosphate that is at least 0.3 M and at least one water-soluble organic amine having a boiling point at atmospheric pressure of at least about 150° C.

### Claim 15 (depends on 14)

The method of claim 14 wherein the water-soluble organic amine is selected from the group consisting of alkanolamines, polyetheramines, and mixtures thereof.

### Claim 16 (depends on 1)

The method of claim 1 wherein the anodizing solution is comprised of water and a concentration of silicon atoms in the form of alkali metal silicate that is at least about 0.4 M.

### Claim 17 (depends on 16)

The method of claim 16 wherein said pulsed current has an average voltage of not more than 75 volts.

### Claim 18 (depends on 1)

The method of claim 1 wherein the anodizing solution is comprised of water and a complex fluoride selected from the group consisting of H2TiF6, H2ZrF6, H2HfF6, H2SiF6, H2GeF6, H2SnF6, H2GeF6, H3AlF6, HBF4 and salts and mixtures thereof.

### Claim 19 (depends on 18)

The method of claim 18 wherein the anodizing solution is additionally comprised of HF or a salt thereof.

### Claim 20 (depends on 18)

The method of claim 18 wherein the anodizing solution is additionally comprised of a chelating agent.

### Claim 21 (depends on 18)

The method of claim 18 wherein the anodizing solution is additionally comprised of an amine, ammonia, or mixture thereof.

### Claim 22

A method of forming a protective coating on a surface of a metallic article comprised of aluminum, magnesium or a mixture thereof, said method comprising:
A) providing an anodizing solution comprised of water and a concentration of phosphorus atoms in the form of phosphate that is at least 0.3 M but essentially free of ammonia, chromium, permanganate, borate, sulfate, free fluoride and free chloride;
B) providing a cathode in contact with said anodizing solution;
C) placing said metallic article as an anode in said anodizing solution; and
D) passing a pulsed direct current having an average voltage of not more than 100 volts between the anode and the cathode for a time effective to generate a visible light-emitting discharge and form said protective coating on said surface.

### Claim 23 (depends on 22)

The method of claim 22 wherein said anodizing solution is additionally comprised of a water-soluble amine selected from the group consisting of alkanolamines, polyether amines, and mixtures thereof.

### Claim 24 (depends on 23)

The method of claim 23 wherein said anodizing solution is comprised of at least about 0.05 M of said water-soluble amine.

### Claim 25 (depends on 22)

The method of claim 22 wherein said pulsed direct current has an average voltage of not more than 60 volts.

### Claim 26 (depends on 22)

The method of claim 22 wherein said anodizing solution is comprised of a concentration of phosphorus atoms in the form of phosphate that is at least 0.5 M.

### Claim 27 (depends on 22)

The method of claim 22 wherein said phosphate is comprised of a potassium salt of phosphoric acid.

### Claim 28

A method of forming a protective coating on a surface of a metallic article comprised of aluminum, magnesium or a mixture thereof, said method comprising:
A) providing an anodizing solution comprised of water and a water-soluble silicate;
B) providing a cathode in contact with said anodizing solution;
C) placing said metallic article as an anode in said anodizing solution; and
D) passing a pulsed direct current having an average voltage of no more than 100 volts between the anode and the cathode to generate a visible light-emitting discharge and to form said protective coating on said surface.

### Claim 29 (depends on 28)

The method of claim 28 wherein the anodizing solution contains a concentration of silicon atoms in the form of silicate that is at least about 0.4 M.

### Claim 30 (depends on 28)

The method of claim 28 wherein the anodizing solution is essentially free of ammonia, chromium, permanganate, borate, sulfate, free fluoride and free chloride.

### Claim 31

A method of forming a protective coating on a surface of a metallic article comprised of aluminum, magnesium or a mixture thereof, said method comprising:
A) providing an anodizing solution comprised of water and a water-soluble complex fluoride of an element selected from the group consisting of Ti, Zr, Hf, Si, Sn, Al, Ge, B and combinations thereof,
B) providing a cathode in contact with said anodizing solution;
C) placing said metallic article as an anode in said anodizing solution; and
D) passing a pulsed direct current having an average voltage of not more than 125 volts between the anode and the cathode for a time effective to generate a visible light-emitting discharge and to form said protective coating on said surface.

### Claim 32 (depends on 31)

The method of claim 31 wherein the complex fluoride comprises an anion comprising at least 4 fluorine atoms and at least one atom selected from the group consisting of Ti, Zr, Si, and combinations thereof.

### Claim 33 (depends on 31)

The method of claim 31 wherein the complex fluoride is selected from the group consisting of H2TiF6, H2ZrF6, H2SiF6, and salts and mixtures thereof.

### Claim 34 (depends on 31)

The method of claim 31 wherein said complex fluoride is present in the anodizing solution at a concentration of at least 0.1 M.

### Claim 35 (depends on 31)

The method of claim 31 wherein the anodizing solution is additionally comprised of hydrofluoric acid, a salt of hydrofluoric acid, or a mixture thereof.

### Claim 36 (depends on 31)

The method of claim 31 wherein the anodizing solution is additionally comprised of a chelating agent.

### Claim 37 (depends on 31)

The method of claim 31 wherein the anodizing solution is additionally comprised of at least one compound which is an oxide, hydroxide, carbonate or alkoxide of at least one element selected from the group consisting of Ti, Zr, Si, Hf, Sn, B, Al and Ge.

### Claim 38 (depends on 31)

The method of claim 31 wherein the anodizing solution has a pH of from about 3 to about 11.

### Claim 39

A method of forming a protective coating on a surface of a metallic article comprised of aluminum, magnesium or a mixture thereof, said method comprising:
A) providing an anodizing solution, said anodizing solution having been prepared by dissolving a water-soluble complex fluoride of an element selected from the group consisting of Ti, Zr, Hf, Si, Sn, Ge, B and combinations thereof and an inorganic acid or salt thereof that contains fluorine but does not contain any of the elements Ti, Zr, Hf, Si, Sn, Ge or B in water and said anodizing solution having a pH of from about 3 to about 11;
B) providing a cathode in contact with said anodizing solution;
C) placing said metallic article as an anode in said anodizing solution; and
D) passing a pulsed direct current having an average voltage of not more than 125 volts between the anode and the cathode for a time effective to generate a visible light-emitting discharge and form said protective coating on said surface.

### Claim 40 (depends on 39)

The method of claim 39 wherein the pH of the anodizing solution is adjusted using ammonia, an amine, an alkali metal hydroxide or a mixture thereof.

### Claim 41 (depends on 39)

The method of claim 39 wherein the inorganic acid is hydrogen fluoride or a salt thereof;

### Claim 42 (depends on 39)

The method of claim 39 wherein the anodizing solution is additionally comprised of a chelating agent.

### Claim 43 (depends on 39)

The method of claim 39 wherein the anodizing solution is additionally comprised of at least one compound which is an oxide, hydroxide, carbonate or alkoxide of at least one element selected from the group consisting of Ti, Zr, Si, Hf, Sn, B, Al and Ge.

### Claim 44

A method of forming a protective coating on a surface of a metallic article comprised of aluminum, magnesium or a mixture thereof, said method comprising
A) providing an anodizing solution comprised of water and a water-soluble permanganate;
B) providing a cathode in contact with said anonizing solution;
C) placing said metallic article as an anode in said anodizing solution; and
D) passing a pulsed direct current having an average voltage of not more than 200 volts between the anode and the cathode for a time effective to generate a visible light-emitting discharge and form said protective coating on said surface.

### Claim 45 (depends on 44)

The method of claim 44 wherein the anodizing solution is additionally comprised of a mineral acid.

### Claim 46 (depends on 44)

The method of claim 44 wherein said water-soluble permanganate is present in the anodizing solution at a concentration of at least about 0.01 M.

### Claim 47

A method of forming a protective coating on a surface of a metallic article comprised of aluminum, magnesium or a mixture thereof, said method comprising
A) providing an anodizing solution, said anodizing solution having been prepared by dissolving a water-soluble complex fluoride of zirconium or salt thereof and an oxide, hydroxide, carbonate or alkoxide of zirconium in water and said anodizing solution having a pH of from about 3 to 5;
B) providing a cathode in contact with said anodizing solution;
C) placing said metallic article as an anode in said anodizing solution; and
D) passing a pulsed direct current having an average voltage of not more than 125 volts between the anode and the cathode for a time effective to generate a visible light-emitting discharge and form said protective coating on said surface.

### Claim 48 (depends on 47)

The method of claim 47 wherein H2ZrF6 or a salt thereof is used to prepare the anodizing solution.

### Claim 49 (depends on 47)

The method of claim 47 wherein zirconium basic carbonate is used to prepare the anodizing solution.

### Claim 50 (depends on 47)

The method of claim 47 wherein the pH of the anodizing solution is adjusted using a base.

### Claim 51 (depends on 47)

The method of claim 47 wherein the anodizing solution has been prepared by dissolving about 0.1 to about 1 weight percent zirconium basic carbonate and about 10 to about 16 weight percent H2ZrF6 or salt thereof in water and adding a base if necessary to adjust the pH of the anodizing solution to between about 3 and about 5.

### Claim 52

A method of forming a protective coating on a surface of a metallic article comprised of aluminum, magnesium, or a mixture thereof, said method comprising:
A) providing an anodizing solution comprised of water and a water-soluble compound selected from the group consisting of titanates, zirconates, and mixtures thereof;
B) providing a cathode in contact with said anodizing solution;
C) placing said metallic article as an anode in said anodizing solution; and
D) passing a pulsed direct current having an average voltage of no more than 150 volts between the anode and the cathode to generate a visible light-emitting discharge and to form said protective coating on said surface.

### Claim 53 (depends on 52)

The method of claim 52 wherein the anodizing solution is comprised of water-soluble zirconium carbonate.

### Claim 54 (depends on 52)

The method of claim 52 wherein the anodizing solution is comprised of zinc ammonium zirconium carbonate.

### Claim 55 (depends on 52)

The method of claim 52 wherein the anodizing solution is comprised of a decavanadate.

### Claim 56 (depends on 55)

The method of claim 55 wherein the anodizing solution is additionally comprised of a chelating agent.

### Claim 57 (depends on 55)

The method of claim 55 wherein the anodizing solution has a pH of from 11 to 14.

### Claim 58

A method of forming a protective coating on a surface of a metallic article comprised of aluminum, magnesium or a mixture thereof, said method comprising
A) providing an anodizing solution comprised of water and a water-soluble alkali metal fluoride;
B) providing a cathode in contact with said anodizing solution;
C) placing said metallic article as an anode in said anodizing solution; and
D) passing a pulsed direct current having an average voltage of not more than 125 volts between the anode and cathode through said anodizing solution for a time effective to form said protective coating on said surface.

### Claim 59 (depends on 58)

The method of claim 58 wherein the water-soluble alkali metal fluoride is potassium fluoride.

### Claim 60 (depends on 58)

The method of claim 58 wherein said anodizing solution is comprised of about 15 to about 45 g/L potassium fluoride, less than 0.5 g/L hydroxide, and less than 1 g/L silicate.

### Claim 61

A method of forming a protective coating on a surface of a metallic article comprised of aluminum, magnesium or a mixture thereof, said method comprising:
A) providing an anodizing solution comprised of water and a water-soluble alkali metal hydroxide;
B) providing a cathode in contact with said anodizing solution;
C) placing said metallic article as an anode in said anodizing solution; and
D) passing a pulsed direct current having an average voltage of not more than about 100 volts between the anode and cathode through said anodizing solution for a time effective to form said protective coating on said surface.

### Claim 62 (depends on 61)

The method of claim 61 wherein the water-soluble alkali metal hydroxide is potassium hydroxide.

### Claim 63 (depends on 61)

The method of claim 61 wherein said anodizing solution is comprised of from about 0.1 to about 1.1 M alkali metal hydroxide.